      In reference to https://www.finishing.com/64/34.shtml :

      The scratches are still there because the 150-grit disk cuts far deeper than the non-woven disk can repair. Non-woven pads refine a surface; they do not remove coated-abrasive scratches. That is the whole selection rule: the coated stage before the pad must finish at least one grade finer than feels necessary.

      For 304 welds on 2B sheet, a reliable sequence is: level the weld with the 150-grit disk, then refine with 220 grit on the orbital sander before the non-woven pad ever touches the part. Only then go to a medium non-woven disk for blending, and finish with a fine non-woven disk if the surrounding sheet needs it. The 220 step is the one most shops skip, and it is the reason weld ghosts keep showing up after the pad work.

      Two more details matter. First, remove heat tint before blending, either mechanically or with pickling paste, because discoloration under a satin finish reads as a defect no pad can hide. Second, run the non-woven disk with light, steady pressure and overlapping passes in one consistent direction. Heavy pressure collapses the open web structure that makes these pads work. The fibers are meant to flex and present fresh mineral as they wear, which is what produces the uniform scratch pattern.

      If the 7-inch disk keeps leaving deep marks, switch weld leveling to a flap disc in 120 grit. It cuts cooler and leaves a shallower scratch that the 220 step erases quickly.