      Lines that appear only at certain angles are scratches, not smears. A smear wipes off; a scratch catches raking light. Wipe the part with mineral spirits and look at it under a single bright light held low to the surface. If the lines are still there, they are scratches left by an earlier step that your final compound never removed.

      The usual cause is a skipped grade. Buffing compounds cut very little. If you go from a coarse cutting stage straight to a fine coloring compound, the fine compound cannot erase the coarse scratches, so they stay visible as lines that shift with the viewing angle. The fix is to step back, not to buff harder. Re-sand or re-cut at the finest grade that still shows a uniform scratch pattern, then work forward through every intermediate stage.

      Three shop habits prevent this. One, dedicate one wheel to one compound and never mix them. A speck of coarse compound embedded in a finishing wheel will re-scratch the part on every pass. Two, clean the part with solvent between stages so stray grit from the last step does not travel forward. Three, keep pressure light on the final passes and let the compound do the work. On aluminum especially, heavy pressure smears the surface and leaves the streaks you described.

      Once the lines are true scratches, no hand-applied polish will remove them. The only way out is back through the grades.