Viewing 6 posts - 1 through 6 (of 6 total)
  • Author
    Posts
  • #50578
    kmlplater
    Participant

      Hello all,

      We are powder coating very small copper COMM bars and we cannot seem to get the flow right and there are adhesion voids under magnified viewing. We need the COMM Bars to be insulated. We check them with HI-POT and they are failing. We have tried a few pre finish processes to get the Powder Coat to stick better by Electroless nickel plating the COMM bars. The last process we have tried is Caustic Electroclean on Direct>Rinse>HCl>Rinse>x2>Chromic Acid clean>Rinse>Cyanide Copper Strike>Rinse>Acid Nickel Strike>Rinse>High Phos Electroless Nickel for .0002>Rinse>Dry>400 deg oven>Powder coat.

      Can anyone offer any advise that would be an improvement?

      Thanks in Advance

      #50725
      Ted Mooney
      Participant

        Hi, KML.

        I may be misunderstanding something. Do the components require electroless nickel plating or are you doing that only to improve the adhesion?

        The usual pretreatment before powder coating is phosphatization. But because your parts are copper rather steel or zinc, zinc phosphating on copper probably won’t work.

        Have you considered zinc plating the parts, then phosphatizing them before powder coating. Alternately an epoxy powder coating should stick to clean copper.

        But electrophoretic coating, CED, would offer a much thinner but still pore-free coating than powder coating.

        • This reply was modified 4 months ago by Ted Mooney.
        #52013
        kmlplater
        Participant

          Hello Ted,

          Thank you for your response. Reference to your question, I am experimenting with Electroless nickel as well as nickel strike and copper strikes to see which has the best adhesion. I had considered Zinc but I was advised that because of the COMM bars going through High Pot testing there is a greater chance of microscopic voids or trapped moisture. Also, I was wondering if my Electroless Nickel might not be the best option because the solution we are using is High phosphate and that also might to much of a smooth surface for the powder coat to stick on.

          As of right now, because of the size of these small COMM bars, we are going to add a course abrasive in a tumbler instead of sandblast to create a rougher surface with the EN for now. Hopefully that will add the flow result of the powder coat. I also am working on a better way to heat these up in the oven and maintain the heat until we spray them. They are so small they dissipate heat quickly.

          I have not considered an Epoxy powder coat or the CED though. I will bring it up with the engineers.

          #58703
          surfacepolish_max
          Participant

            KML, there is a contradiction in the plan you described at the end that I think is worth resolving before you spend more time on it, because it may be working against you.

            Your problem is not adhesion in the cosmetic sense. You are failing HI-POT, which means the coating has to be electrically continuous over the whole surface, including edges, corners and any thin spots. That makes this a coverage-and-continuity problem, not a roughness problem.

            The plan you described – adding a coarse abrasive in a tumbler to roughen the electroless nickel so the powder grips better – is likely to make HI-POT worse rather than better. Roughening the substrate gives you mechanical keying, which helps peel and impact adhesion, but it does not help electrical continuity. What it does do is create a topography with peaks that can end up with thinner powder over them and valleys that can trap air, and it introduces abrasive residue and smeared metal into the surface that you then have to remove completely before coating. On a part whose acceptance test is dielectric breakdown at every point, you want the smoothest, most defect-free, most uniform substrate you can get – not the roughest.

            A few things I would separate:

            1. Which layer is actually failing. Before changing the pretreatment again, break a failed part down and find out whether the breakdown is at the copper/EN interface, inside the EN, at the EN/powder interface, or through a thin or pinhole region of the powder. HI-POT failure tells you there is a conductive path, not where it is. If you can section a failed part, or test the EN-coated part before powder coating with the same HI-POT method, you will learn immediately whether the EN is already discontinuous or whether the powder is the problem. Testing the EN-coated part on its own is the cheapest and most decisive step available to you, and it is worth doing before any more process changes.

            2. High-phos EN is the right instinct, but for the wrong reason. High-phosphorus EN is more corrosion resistant and less porous than mid or low phos, which is what you want for a barrier layer. But it is also smoother and has a different surface chemistry, and powder does not bond to it as readily as to a properly prepared metal surface. So it makes a better barrier and a harder-to-bond surface at the same time. If EN is genuinely needed for electrical reasons, then treat the EN surface as the substrate that must be prepared for coating – and prepare it chemically (a controlled etch or a suitable pretreatment matched to EN) rather than by blasting it with coarse abrasive.

            3. Edges and coverage. Small parts with edges, plus a coating applied over a part that cools fast, is a classic setup for thin coverage on edges and corners. Powder tends to thin at edges and you get exactly the pinhole and continuity failures you are seeing. This is worth checking directly: coat a small batch, then inspect edges specifically at magnification, and compare edge coverage against the flat faces. If edges are the failure sites, the fix is in the application and the part handling (heating, racking, avoiding cooling between spray and cure), not in the pretreatment chemistry.

            4. What Ted suggested and I would second. Electrophoretic coating (CED/e-coat) gives a much thinner but far more uniform and pore-free film than powder, and by its nature it covers edges and recesses better because it deposits by current and self-limits. For an insulation requirement verified by HI-POT on small parts, an e-coat is usually a better process fit than powder. If the engineers will consider it, that is likely the shortest route to passing the test rather than fighting powder flow.

            The heat point you raised is real and important. Parts this small lose heat quickly, and if the substrate is below the temperature the powder needs at the moment of deposition, you get poor flow and incomplete fusion regardless of pretreatment. Improving how you hold and transfer heat between oven and spray is a genuinely good instinct, and I would keep that work.

            Disclosure: I work for a manufacturer of vibratory and mass finishing equipment, so I am answering from surface-preparation and surface-condition experience rather than as a plating line chemist or a powder coating supplier.

            Max Xu
            Surface Finishing Engineer, SurfacePolish

            #58726
            ZhangSheng
            Participant

              Hi KML,

              A few process-side observations from running small copper parts through powder:

              1. Grounding is everything on small parts. Poor ground contact is the most common cause of weak transfer and bad flow on small pieces — the charge leaks away before the powder can build. Make sure every bar has a clean, solid ground path through the hook/rack (scrape the contact points, check ground continuity regularly). Small geometry also gives you Faraday cage effects; dropping gun voltage and powder output and spraying a bit farther back usually improves coverage more than turning things up.

              2. For hi-pot, film continuity matters more than the resin type. Pinholes fail hi-pot long before adhesion does. Check your actual DFT — for ~1 kV you want a continuous film, typically on the order of 60-80+ microns with no thin spots at edges and corners (edges pull powder thin). Sharp edges are pinhole magnets; even a small edge radius helps a lot.

              3. Copper is tricky because it conducts heat away so fast. Small bars can pass through the oven without the substrate itself reaching full cure temperature for the required time, which shows up as poor flow and weak adhesion. Put a thermocouple on an actual part (not just oven air) and confirm time-at-temperature against the powder’s cure schedule. A preheat pass also drives off adsorbed moisture, a classic pinhole source on copper.

              4. Your EN-underlayer instinct is sound. A thin electroless nickel layer (a few microns is plenty — it is just an adhesion key here, and being metallic it will not hurt conductivity at contact areas) gives the powder something consistent to bite on, versus bare copper that re-oxidizes in minutes. Keep the transfer from EN rinse to the powder booth dry and quick, and go easy on the tumbling idea — coarse media can peen through or contaminate a thin EN layer.

              5. One practical note since these are electrical bars: any contact or termination area that must stay conductive has to be masked before powder, because the cured film is an insulator. Use a polyester (green) high-temperature tape with a silicone adhesive, and check the adhesive’s continuous temperature rating against your cure cycle (typically 180-200 C for powder), not just the film itself. Apply it to a clean, dry surface and press the edges down firmly so powder cannot creep underneath; remove it at the temperature the tape maker specifies (some are hot-peel, some cold-peel) to avoid adhesive residue on the contacts.

              If you can share your measured DFT range and cure profile, it is easier to tell whether this is a coverage problem or a cure problem.

              Zhang Sheng

              #58740
              surfacepolish_max
              Participant

                I would start by separating two failures that are easy to merge, because they point in opposite directions.

                Adhesion voids and HI-POT failure are not the same problem. An adhesion void is an interface issue – cleanliness or wetting under the film. A HI-POT failure is dielectric integrity of what is already on the part – a pinhole or a thin spot conducting through. It is entirely possible to have excellent adhesion and still fail HI-POT, which is what I would expect on a 0.0002 inch high-phosphorus electroless nickel layer over copper. Chasing pre-treatment for a dielectric problem will keep missing.

                The cheapest way to split them is one control batch: take bars through the electroless nickel exactly as now, skip the powder, and run HI-POT on the bare EN. If bare EN fails, the powder is irrelevant and the work belongs on the nickel – thickness at the thinnest point, not the average, and porosity. If bare EN passes and EN plus powder fails, the work belongs at the powder interface and you save yourself the whole plating investigation. One batch answers which half to work on.

                Two things from our side that are specific to bars this small:

                • Flow is usually geometry and heat, not pre-treatment. On very small parts the powder has less time to level before gel and cure because the part’s thermal mass is low, and Faraday effects at edges and thin sections thin the film exactly where voids show. No pre-treatment improves that. If the voids sit on edges and thin sections, look at gun geometry, kv and part rotation or grounding rather than at the plating sequence.
                • Contact between small parts is a coating killer. Bars that touch each other through plating, drying and coating mask each other at the contact point, and the masked spot is both a thin dielectric and a future void. We see this constantly in small-part work: loading method, part-to-part contact and separation before coating change the result far more than most chemistry changes. Barrel or vibratory handling with complete separation of media and parts before the powder booth removes a whole class of these spots.

                One question rather than a claim, since I may be missing the intent: what is the 400 degree oven for? If it is there to dehydrate or outgas the nickel before powder, it may be doing the opposite of what you want, because driving adsorbed moisture off a thin deposit can leave the voids you are then finding under magnification. If it is there for stress relief, it is worth confirming that the high-phosphorus layer behaves the way you expect after heating, since that layer is normally applied and used as-deposited.

                To be clear about my own limits: we build mass-finishing equipment and media, not electroless nickel or powder chemistry, so I am not going to advise changing your plating stack. What I am confident about is the split between adhesion and dielectric, and the control batch that tells you which one you actually have.

              Viewing 6 posts - 1 through 6 (of 6 total)
              • You must be logged in to reply to this topic.