Home of The Finishing HOTLINE since 1989 › Forums › 2. Metallic Finishing › Black Oxide, Bluing, Coloring, Patinas › Issues finding a trivalent chromate that does not require nitric acid

Viewing 5 posts - 1 through 5 (of 5 total)
  • Author
    Posts
  • #58602
    Timothy
    Participant

      Hello,

      Currently, I have been trying to get my company to start doing rack Zinc black. The issue I am facing is on the line this would be going we have two clear chromates, one of which is used for 1 family of parts because it doesn’t use nitric and we have found that nitric causes the bore hole areas of this family of parts to rust almost immediately after application. I have done research on multiple different suppliers and have not found a suitable replacement, and I have not been able to trial other parts on the same line to go through the non-nitric chromate and see how it affects the quality of the part.

      The process we do on this line is Zinc chloride and alkaline zinc, so I would need something compatible with both. The chromates we are using are from the Atotech family.

      Any assistance in this matter would be greatly appreciated

      #58609
      Forum Admin
      Keymaster

        There are black trivalent passivates whose suppliers claim compatibility with both acid and alkaline zinc. MacDermid Enthone describes TriPass ELV 5300 as designed for both deposits, with a topcoat or post-dip recommended. See MacDermid Enthone TriPass ELV 5300.

        Columbia Chemical’s TRIVECTA BLACK 300 technical data sheet also lists acid chloride and alkaline cyanide-free zinc, although it recommends a dilute nitric acid pre-dip. See the TRIVECTA BLACK 300 technical data sheet. Metalline ZnB is another supplier-listed process for acid and alkaline zinc, but it uses a proprietary Preblack conditioner. See Metalline ZnB.

        I could not verify from official literature that any of these black processes can operate without nitric acid or another activation step. I would ask each supplier for written confirmation covering your exact chloride and alkaline zinc bath identities, the required activation, and performance on recessed areas.

        Before concluding that nitric acid is the root cause, I would investigate two other possibilities:

        1. Zinc coverage inside the bore. Recessed and blind areas receive lower current density and may have very thin zinc or no zinc. Plating and passivation problems commonly appear first in these areas. Columbia specifies a minimum zinc thickness of 8 microns for its black system.
        2. Solution entrapment. Bores can carry activation or plating solution into subsequent tanks. Residual salts can remain corrosive after drying because they are hygroscopic.

        One possible explanation, not yet proven, is that the nitric activation is removing marginal zinc from an already thinly plated bore, or that acid remains trapped there and attacks exposed steel. In that case, nitric acid may be revealing an inadequate zinc-coverage or rinsing problem rather than being the sole root cause. Changing only the black passivate might not solve the failure.

        Questions I would want answered include:

        • Are the bores blind or through?
        • What is the measured zinc thickness inside the bore compared with the exterior?
        • Which exact Atotech zinc and clear-passivate products are being used?
        • How many rinses follow plating and activation?
        • Can the rack orientation completely fill and drain the bores?
        • Does the non-nitric clear process remain rust-free after 24 to 48 hours or salt-spray testing?
        • What white-rust and red-rust specification must the black finish meet?

        I would trial candidate black systems on actual parts from both zinc baths, using the supplier-prescribed activation and sealer. Change one variable at a time and record the bore and exterior results separately.

        Additional discussion of zinc coverage and solution entrapment in blind or threaded holes can be found here: Zinc plating blind holes and threaded holes.

        I have added a report here CLICK LINK FOR REPORT

        #58693
        surfacepolish_max
        Participant

          Timothy,

          The Admin has pointed you at the passivate chemistry, which is the right place to start. What I would add is that the observation you already made – that nitric causes the bore holes to rust almost immediately – is a very specific clue, and it is worth reading it as a rinsing and entrapment problem as much as a chemistry problem. That distinction matters, because if it is entrapment, changing the passivate supplier alone will not fix it.

          Consider what happens in a bore during a rack zinc line. The bore fills during each immersion and drains slowly. Nitric-bearing passivate is aggressive, and if it stays in contact with the zinc inside the bore for longer than it does on the outer surfaces, you get two effects at once: the coating inside the bore is thinned or stripped relative to the outside, and the rinse that follows has to remove a harder-to-reach residue. If the rinse does not fully exchange the liquor in the bore, you are left with a dilute acid film sitting against a thinned zinc layer. That is a good recipe for the rapid red rust you describe, and it explains why it appears in bores specifically and not across the whole part.

          Three checks I would run before changing chemistry.

          First, confirm the differential. Take a part straight off the line and, without any further treatment, break it and inspect the bore surface against the outer surface. If the bore coating is visibly thinner, discoloured, or absent, the issue is residence time and exchange in the bore, not the passivate being fundamentally unsuitable. A simple thickness check inside the bore versus the flat will settle this quickly.

          Second, time the drainage. Remove a racked part and watch how long liquor continues to drain from the bores. If it is still draining when the part reaches the next tank, the bore is carrying passivate into your rinse, and the rinse is being asked to do work it cannot do in the dwell time available. Options here are mechanical rather than chemical: rack orientation so bores drain downward rather than filling, a longer drain dwell, an air knife or directed spray into the bore, or a two-stage rinse where the first stage is deliberately short and the second is clean. On many lines a simple rack reorientation removes a problem that no chemistry change will.

          Third, check whether the bores are being adequately wetted at all at the passivate stage. If the bore is small enough that surface tension keeps the passivate from fully entering, then the inside is effectively unpassivated zinc, and it will rust regardless of which trivalent system you use. That is a wetting and agitation question, and it is worth confirming because it changes the remedy entirely.

          On the chemistry side, since the Admin has named two candidates, the question I would put to any supplier is not just “is it compatible with both acid and alkaline zinc” but “what is the recommended rinse and dwell sequence after it, and does it tolerate a slower-draining part geometry.” A passivate that performs well on flat panels can behave quite differently on parts with deep bores, and the technical data sheet rarely addresses that. If you can get a sample to trial, run it on the problem family first, not on an easy part – the whole point is to find out whether it removes the bore sensitivity.

          One caution on topcoats. A topcoat or post-dip can mask a bore-rinsing problem by sealing over the residue, and it can look like a fix on a salt spray test while the underlying issue remains for parts that see abrasion or thermal cycling. If you do add a topcoat, I would still fix the rinsing first so that the topcoat is protecting good passivate rather than sealing in a defect.

          I disclose that I work for a surface finishing supplier (SurfacePolish). I have no product to recommend in this thread and no interest in which brand you select – the points above are the checks I would run on our own line before I spent money on a new passivate.

          If you can share the bore diameter and depth, and roughly how long the rack dwells between tanks, that would help narrow which of the three mechanisms is at work.

          #58731
          jamesle
          Participant

            Good points on chemistry and rinsing above — I’d add measurement, since bores lie. Map zinc thickness inside the bore vs the exterior with XRF on the part; rack zinc often plates the bore at half the exterior thickness, and no passivate fixes thin zinc. Log white vs red rust separately per ASTM B117 during trials, changing one variable at a time. Our QC flow: https://www.yumeihardware.com/ Disclosure: I’m with Yumei Hardware.

            #58758
            ESPRONick
            Participant

              Timothy,

              Nitric in a trivalent black does two jobs, it oxidises the film and it lifts the last bit of zinc so the colour comes up dark. Take it out and most suppliers give you peroxide or persulphate instead.Those are out there, you just have to be blunt with the tech rep and ask for the nitric free black, not the standard one.

              Before you swap products though I would look at the bores. Nitric residue sitting in a blind hole will rust the zinc overnight no matter what passivate you use, and a bore that does not drain is a rinse problem, not a chemistryproblem.

              • Rack the parts so the bore sits vertical, or at least on a slope. Sounds obvious, almost nobody does it.
              • Two stage rinse after passivate with real flow, and give the rack 20 to 30 seconds to drain over the tank before it moves.
              • A short dip in dilute NaOH at pH around 9 after the rinse. That kills the acid hiding in the bore. Then one DI rinse and straight to dry.
              • Dry hot, 60 to 70 C, with air moving through the bore. Cold parts with wet bores will flash rust in the rack.

              Your planting line may also be dragging alkaline zinc into the passivate. Check the rinse before the chromate, if the pH is above 8 you are fighting the bath all day.

              Hope that helps. Rack zinc black is fussy but it is doable on a normal line.

            Viewing 5 posts - 1 through 5 (of 5 total)