  • #58671
    Mannanan
    Participant

      Hello folks,

      I am having problems getting a 168 hr salt spray pass on 2014A T4 SURTEC 650V coated panels with BONDERITE C-IC SMUTGO NCB AERO as the deoxidiser. Previously we used BONDERITE C-IC SMUTGO 1 AERO. This is now unavailable to us thanks to REACH. the new version is hexavalent chrome free, being based on diiron tris sulphate, nitric acid potassium nitrate and hydrofluoric acid. I have done many trial combinations around dwell time in the deoxidiser, and others using the old deoxidiser. I get good salt spray passes with the old deoxidiser, but we are required to move on from that. I need a non-hexavalent chrome deoxidiser that works. Any ideas?

       

      #58672
      rh24probert
      Participant

        2014 is touchy, hope it is not heat treated. All companies have a ferric sulfate based deox that works well ahead of the Sur-Tec, just be sure it is air agitated to keep ferric from going ferrous. I can name the specific product but not here. I used the ferric based product ahead of Seu-Tec for 15 years, no problem.

        #58673
        Mannanan
        Participant

          Thaqnk you Robert for your reply, most appreciate that you took the time to help me.

          I will get air agitation put on the tank.

          It makes sense, as the rinses are agitated and they turn red rust coloured when used prior to flushing through with fresh water.

          Best regards

          Mark

          #58674
          rh24probert
          Participant

            Just in case deox was not  the whole problem with the tri-chromate be reminded that the chromate may not be right. pH adjustment is critical, you must dilute the NaOH and add with vigorous agitation or you precipitate some of the product.

            #58675
            Mannanan
            Participant

              Thanks again Robert.

              Looking at the TDS for the none chrome Smutgo, there is no pH to keep it to.

              Also there is a comment about air agitation being merely recommended, and not essential as you would advise.

              TDS could be better sometimes.

              Best regards

              Mark

              #58676
              rh24probert
              Participant

                I cite the pH for the SerTec Chromate 650 , it is very critical hat you dilute the NaOH and add it with vigorous agitation.

                I do not know Smut-Go, But all ferric sulfate deox has to be air agitated to keep the Ferric from going Ferrous. We need to talk, call, me.

                #58678
                Mannanan
                Participant

                  Hi Robert,

                  Arh yes, the pH of the Surtec.

                  We check that daily.

                  Best regrads

                  Mark

                  #58691
                  surfacepolish_max
                  Participant

                    Mark,

                    Robert has given you the key point already, so I will add only what might help you close the gap on the 168 hour salt spray result.

                    Two things in your description stand out as worth checking before you change the deoxidiser again.

                    The first is the ferric/ferrous equilibrium Robert raised. On a diiron tris sulphate based deoxidiser, air agitation is not a nice-to-have refinement, it is what keeps the iron in the ferric state. Your observation that the rinse turns red rust coloured is consistent with ferrous iron carrying over. If ferrous iron reaches the SurTec 650V bath or the surface, you can get iron deposited on the aluminium rather than removed from it, and iron on an aluminium surface is a very effective way to fail salt spray while every bath parameter looks correct on paper. Worth confirming the deoxidiser is genuinely being agitated across the whole tank volume and not just at the point of air entry, because dead zones in a tall narrow tank are common and the TDS wording you quote would not tell you that.

                    The second is the 2014A T4 substrate itself. 2014 is a copper-bearing alloy and it is unforgiving. Copper-rich intermetallic phases at the surface behave differently from the matrix in both the deoxidiser and the subsequent conversion coating, and smut removal that is adequate on 6061 or 5052 is frequently incomplete on 2014. If any smut or copper-enriched layer survives the deoxidiser, the 650V will form over it and the coating will be locally defective in a way that shows up as pitting in salt spray rather than as a uniform coating failure. A useful diagnostic is to compare a 2014A panel against a 6061 or 5052 panel run through the same line on the same day. If the 6000 or 5000 series panel passes and the 2014A fails, the problem is substrate-specific prep rather than the deoxidiser chemistry as such.

                    On the practical side, with a hexavalent-chrome-free ferric sulphate deoxidiser you generally have less process window than the old chromated product gave you. That means dwell time, temperature and concentration each matter more, and the interaction between them matters more than any one of them. If your trials have varied dwell time alone while holding the others, it may be worth a small designed trial that changes concentration and temperature together at two dwell times, so you can see whether you are outside the window entirely rather than just at the wrong end of it.

                    I do not have experience with the specific SMUTGO grades, so treat this as points to check rather than a recommendation – Robert is clearly the person with direct experience here and his offer to talk is worth taking up.

                    One thing I would avoid is adding a mechanical abrasion step to compensate. It can improve appearance and even adhesion short term, but it changes the surface you are then trying to chemically deoxidise, and it makes the result harder to control lot to lot.

                    I disclose that I work for a surface finishing supplier (SurfacePolish). I am not recommending any product here and I have no interest in your deoxidiser choice – I am only offering the substrate and iron-carryover angles because they are the usual suspects when 2014 fails while everything else passes.

                    #58697
                    Mannanan
                    Participant

                      Hi Robert, I missed your invitation to talk directly.

                      How do i contact you, and what is the best time for you.

                      I am on British Summer time, so about 5 hrs ahead of your time.

                      Thanks and best regards

                      Mark

                      #58698
                      Mannanan
                      Participant

                        Hello, Max,

                        thanks for your excellent and comprehensive reply, i very much appreciate the time you have taken to reply to my problem.

                        I have done further trials with air agitation.

                        There has been an improvement, in that there are slightly fewer pits, but its still afail.

                        I take your point about the amount of agitation, and will increase that.

                        Also, the possibility of iron carry over, i shall observe the operator and put in an extra clean rinse stage if need be.

                        I will do some trials with some 6000 series panels, as you say, 2000 series is notorious for this sort of problem.

                        If have varied dwell time in the deoxidiser between, 2 mins, 5 mins, 10 mins, 15 mins and 20 mins.

                        I have found that the shorter times give fewer pits after salt spray, but not a pass.

                        I also did one set with no deoxidiser, that was no good either.

                        Do you think it worth trying 1 min and 30 second dwell times?

                        Thanks again for your attention to this.

                        Best regards

                        Mark Lees

                        In the Isle of Man, a forsaken island in the Irish sea between the UK and Ireland.

                         