    llary
    Participant

      Hi, I run a vinyl record pressing plant and the manufacturing process starts with silvering a nitrocellulose lacquer coated aluminum disc (‘lacquers’) before electroforming in a nickel sulfamate bath.

      We have had an ongoing intermittent problem with milky clouding/staining that is almost always visible under a strong light, or sometimes to the naked eye. The issue is most obvious in the mirror part of a disk or when test plating with a blank disk.

      I suspect the issue is happening at the silvering stage but I can’t be 100% sure this is the only problem. I will give a quick overview of the silvering process and happy to answer any follow up questions or take on board any ideas/suggestions.

      Silvering is done with an automatic spray booth having a fine atomizing dual spray gun for reducer/silver, and separate nozzles for adjustable low/high pressure DI water and other chemicals. The lacquer is washed with RBS35 or liquinox detergent, then a weak HCl acid wash to neutralize the RBS35 followed by DI water, then sprayed with a sensitizing film of stannous chloride. Finally the surface is sprayed with a silver nitrate solution containing water, NaOH and ammonia. The dual spray head also sprays a carefully calibrated flow of reducer containing water, D-glucose and formaldehyde.

      After silvering the parts are immediately placed into a low current (15A) preplate bath that applies a thin layer of nickel to the soft lacquer at low temperature (under 40C). The parts are then moved to a fast plate bath with a rotating platen and electroformed at 12V/150A for around 90 minutes.

      After the fast plate is finished lacquers are separated from the nickel stamper which at this point weighs around 220g. The finished stamper is then desilvered using a standard ammonia+NaOH desilvering solution.

      #37454
      Forum Admin
      Keymaster

        NOTICE: This answer is a result of a frontier model AI trained in the Legacy Material from Finishing.com and other resources. This is a test to get feedback on this feature. Do not take this answer as professional guidance. We welcome feedback on whether it is helpful and/or accurate. We understand that some people are resistant to this technology, we are testing to see if the information is helpful. Frontier model, AI has reached doctoral-level capabilities in many fields. Again, any constructive feedback would be appreciated.


        My first suspicion would be the chemical silvering sequence, especially chloride/acid carryover and sensitizer control, rather than the nickel sulfamate bath.

        Your silvering chemistry is essentially a Tollens/spray silvering system: ammoniacal silver nitrate is reduced by glucose/formaldehyde onto a sensitized surface. In record manufacturing this is the historic route: lacquer masters are cleaned, sensitized with stannous chloride, rinsed, silvered, then nickel electroformed. There is an older related Finishing.com discussion on plating vinyl records here: How to do Gold Plating of Vinyl Records. A general overview of phonograph record production also describes lacquer silvering followed by nickel electroforming here: Production of phonograph records.

        The “milky clouding” clue is important. Silver chloride is white/milky, and you have several possible chloride sources: the HCl wash and the stannous chloride sensitizer. If either is carried into the silver nitrate spray in excess, you can form AgCl or a mixed silver/silver chloride haze instead of a clean metallic silver mirror. I would especially question whether the HCl “neutralization” step is leaving chloride salts/residue on the lacquer. Neutralizing detergent on the surface is less desirable than fully rinsing the detergent away, then using any acid step as a controlled, separately rinsed treatment.

        I would also verify whether the stannous chloride step is being rinsed correctly. The old record-process descriptions generally include a rinse after SnCl2 sensitizing before the silver/reducer spray. Too little SnCl2 gives poor initiation/skip; too much or poorly rinsed SnCl2 can leave tin/chloride/acid residue and create a gray-white or cloudy silver film. The same basic surface-sensitizing concept is discussed in relation to Tollens/silver mirror chemistry here: Tollens’ reagent.

        Troubleshooting Order

        1. Prove whether the clouding exists before nickel.
          Run a lacquer through cleaning, acid, sensitizer, and silvering only. Do not preplate it. Inspect under the same strong light. If the haze is visible at this stage, the nickel baths are probably only preserving or amplifying a silvering defect.
        2. Run witness panels in parallel.
          Put a clean glass strip or polished plastic witness next to the lacquer during silvering. If the witness is cloudy too, the issue is chemistry, nozzles, water, or spray balance. If only the lacquer clouds, look harder at lacquer cleaning, wetting, surface attack, or residues.
        3. Check chloride carryover.
          After the HCl step and after SnCl2, collect the final DI runoff and test conductivity, pH, and chloride if possible. The final runoff should look like clean DI, not a weak process solution. If chloride is detectable at meaningful levels before silvering, that is a red flag.
        4. Rethink the HCl “neutralization” step.
          RBS35 and Liquinox are good lab detergents, but residues can be stubborn. I would rather see a very thorough DI rinse after detergent, then a controlled acid dip/spray only if the lacquer supplier/process requires it, followed by another thorough DI rinse. Do not rely on acid to “neutralize” detergent residue on the part.
        5. Control SnCl2 age, concentration, acidity, and dwell.
          Stannous chloride oxidizes/hydrolyzes and can become inconsistent. Make it fresh on a schedule, filter if appropriate, keep concentration and acid level constant, and log dwell/spray time. Intermittent clouding often turns out to be “same nominal chemistry, different real chemistry.”
        6. Verify silver/reducer balance at the spray head.
          A dual spray system can look calibrated while still drifting because of nozzle wear, partial blockage, air pressure changes, tubing restriction, check valve behavior, or chemical viscosity/temperature. If reducer is locally high, silver can reduce in the air or as loose particles rather than as a coherent film. If silver/ammonia balance is off, you can get dull gray deposit or precipitation.
        7. Watch DI water quality and rinse mechanics.
          Silvering is unforgiving. DI water should be low conductivity, low in organics if possible, and free of microbial slime. A final rinse that beads, sheets unevenly, or leaves drying marks will often become a silvering defect.
        8. Look for wetting/organic contamination.
          Nitrocellulose lacquer can hold fingerprints, sleeve residues, cutting oils, plasticizer traces, detergent films, and airborne organics. A water-break-free surface before sensitizing is a useful practical check. If the mirror area shows the defect most clearly, that may simply be because the defect is easier to see there, not because grooves are immune.
        9. Do a “fresh chemistry day” test.
          New detergent, new acid, new SnCl2, new silver, new reducer, freshly cleaned nozzles, verified DI. If the problem disappears, reintroduce old variables one at a time.
        10. Do not ignore the preplate, but treat it as the second suspect.
          Nickel sulfamate electroforming baths rely on pH, boric acid buffering, chloride/anode behavior, additives, and wetting agents. Wetting agents help prevent gas bubbles and voids in nickel electroforming, and additive control affects
        • This reply was modified 4 months, 2 weeks ago by Forum Admin. Reason: clarification
        #37578
        Ted Mooney
        Participant

          I was involved in a project different in some ways but similar in many ways: the fresnel lenses used on old style overhead projectors where you would lay a transparency on the projector glass and display the image on a movie screen. Similar because the feature size is not terribly different, and the same silvering and plating is done. Different in that there were only a couple of styles rather than thousands of different recordings. And different because the haze/cloudiness was unacceptably projected onto the silver screen, rather than probably being inaudible on a vinyl disc.

          We found that the main (not only) problem was that soft brushes were occasionally used for cleaning somewhere along the line and even the softest brushes marred the surfaces in a way that was very hard to identify and quantify but caused a haze. If you are sure that no one ever cleans any lacquer, mother stamper, etc.  with a brush move on to Step 2 :-)

          #37768
          llary
          Participant

            Thanks for the follow up. We do in fact use a special brush (sorry, I forgot which exotic animal hair it’s made from but it was expensive!) I have tried some tests today without brushing and we seem to get identical clouding/staining whether the parts were brushed or not.

            The problem today seems particularly bad – I’ve attached some photos below. During the initial stages of the process it looks like the surface is not being thoroughly wetted. As the SnCl is sprayed on there are large water breaks visible on the surface.

            mirror silvering clouding 2

            #37769
            Ted Mooney
            Participant

              It may not actually be the brush which caused the problem I’m familiar with, but the cleaning agent, little particles of TSP or whatever, being brushed around might have acted as an abrasive.  In any case, not brushing solved the problem but that doesn’t seem to be your problem

              I’m not highly experienced with the SnCl2 step before the silvering in record manufacturing, but if you are experiencing water breaks, you obviously have a problem which must be solved since there must be no water breaks. Waterbreak is caused by one of two things, a surface that isn’t truly clean, or an organic surface which water can’t wet without a wetting agent.

              Regarding truly clean, I know that silicone sprays commonly cause ugly problems in plating shops because maintenance personnel don’t realize that normal cleaning processes cannot remove silicone.

              If you’re sure that silicone  sprays are never allowed into the shop, I understand that ethoxylated tallow amine is sometimes used as a wetting agent before two-component silvering … but I honestly don’t know if it’s appropriate in vinyl record production. The purveyors of silvering and activating processes will have familiarity with wetting agents before silvering and may be able to offer advice. Good luck.

               

              • This reply was modified 4 months, 2 weeks ago by Ted Mooney.
              #39137
              llary
              Participant

                Definitely no silicone sprays here and we operate in a cleanroom that’s dedicated to this stamper process.

                I am equally suspicious there is something up with our initial degreasing/wetting and/or there is an issue with the stannous chloride supply.

                The traditional process of stamper production involves using rocker baths first for a detergent like RBS35, then tree saponin used for wetting followed by another rocker bath where the lacquer soaks in the sensitizer for a very specific length of time. Lacquers are then moved to a spray booth for manual or automatic spraying.

                We use a fully automatic process where the entire process is done in the spray booth controlled by a PLC. Back in the day huge plants like Capitol and EMI used a similar process so we are not completely reinventing the wheel, and it worked great until it didn’t.

                I think I will go back to basics and test with the traditional rocker bath method. Also we never saw any difference using saponin so our process skips that step and we seemed to get good wetting regardless. Maybe that’s also something I have to look into again.

                Going to be a fun couple of weeks I guess.

                #44327
                rh24probert
                Participant

                  My experience with sulfamate nickel on duPont silver paint was on the making of floor tile moulds. The customer had brought in a slab of natural Vermont slate, sprayed on the silver paint, and put it directly into the 10 oz/gal nickel sulfamate solution. Starting at zero voltage and zero amperage I spent 30 minutes slowly increasing the voltage  until I saw the target amperage on the amp meter. Then I told them to pull on Saturday after next at 10:30 AM. They called and announced they had a perfect mould 5/8″ thick.

                  First, use Inco S-rounds and y9u will not need any chloride in the solution, othewise limit the chloride to 1/2 oz/gal.

                  At the bottom of the ripple curve the chkoride will attack and/or strip the silver and cause a blemish

                  Ramp up from zero/zero (I hope your rectifier will metee that low.) for at least 30 minutes up to 20 amps / sq foot./

                   

                   

                  #58695
                  surfacepolish_max
                  Participant

                    Your latest observation is the most useful clue in the thread, and I would treat it as the primary lead rather than a side note: <b>large water breaks while the SnCl2 is being sprayed</b> means the lacquer surface is not at a high enough surface energy for the aqueous sensitizer to wet it. On a surface that will not wet, the sensitizer deposits unevenly, silver nucleates unevenly on top of that, and you get exactly the milky, patchy film you describe, worst in the mirror area because that is where an uneven film is easiest to see. So I would stop treating the clouding as a silvering-chemistry problem for now and treat it as a <b>substrate wetting problem that the silvering merely reveals</b>.

                    Two things are worth separating, because they have different fixes.

                    <b>1. Is the surface actually clean, or is it clean but not wettable?</b> These look identical in the booth. On a nitrocellulose lacquer the usual cause of a persistent water break is not visible soil but a <i>mobile</i> layer at the surface: residual detergent that has not been fully rinsed, plasticiser or other low-molecular-weight material migrating out of the lacquer, or a film left by whatever the lacquer was last wiped with. Detergent residue in particular behaves exactly like this – you can rinse until the runoff is clean by conductivity and still have a monolayer left that holds the contact angle high. The reason your acid step does not fix it is that neutralising a detergent does not remove it; neutralised detergent is still a surfactant sitting on the surface, and it is precisely a surfactant film that produces the wetting problem you are seeing.

                    <b>2. How to tell them apart quickly.</b> A water-break test on an unprocessed lacquer disc is the cheapest experiment available. Take a disc, do the rinse exactly as production does, and observe the sheet of water under the same lighting. If it breaks, you have your defect before any chemistry is applied, and nothing downstream can be blamed. Then split it: rinse-only, versus rinse with the acid step, versus rinse with a genuine wetting agent. If a wetting agent gives a continuous sheet and the others do not, you have confirmed a surface-energy problem rather than a cleaning problem.

                    On the specific question of saponin, which you said you dropped because you saw no difference – I would read that result carefully rather than as evidence that saponin is unnecessary. Saponin was in the traditional process as a wetting agent for exactly this stage. “No difference” is what you would expect if your bath method already wet adequately at that time. It is also what you would expect if saponin was added at a point where the damage had already been done. Given that you now have a documented water break, reinstating it is not a step backwards; it is restoring a control that the old process used for the problem you currently have. Your plan to go back to rocker baths is a sound way to test that, because immersion with dwell time wets far more reliably than a spray of fixed volume – if the rocker bath route removes the break, the difference is dwell and wetting, not chemistry.

                    Two practical checks that cost little and often catch this class of fault: verify the final DI runoff conductivity <i>after</i> the last rinse on the disc itself rather than at the drain, and confirm the DI supply has no biofilm or organic loading, since a rinse that beads or dries with marks will become a silvering defect exactly as you describe.

                    Disclosure: I work in surface finishing and polishing, so this is applied surface-preparation reasoning rather than a comment on any specific proprietary silvering or sensitising product – your process suppliers will know the compatible wetting agents for a nitrocellulose substrate.