Chromic acid g/l concentration checking method…
Chromic Acid Analysis – Simple Method
Required Chemicals:
0.1 N Sodium Thiosulphate
Potassium Iodide (KI)
Hydrochloric Acid (HCl)
Starch Indicator
Procedure:
Take 10 mL of Chrome Bath solution.
Dilute it to 500 mL using distilled water.
Take 10 mL of diluted solution in a conical flask.
Add 10 mL of 50% HCl.
Add 10 mL of 10% KI.
Titrate with 0.1 N Sodium Thiosulphate.
Add starch near the endpoint and continue until the blue colour disappears.
Calculation
V = Burette reading in mL.
Example: Burette reading = 15 mL
15 x 16.67 =250.05
November 5, 2026 at 10:39 am #58771shahul,
Your iodometric method is correct for chromic acid. One tweak: a 10 mL to 500 mL dilution is coarse, each drop of thiosulphate swings the number too much. Go 10 mL to 1000 mL, or take a 5 mL sample instead, and the titration gets smooth. Use the same dilution every time or your trend charts are useless.
For the sulphate side, the usual route is barium chloride precipitation and weighing the BaSO4. It is slow but honest. Keep the ratio near 100:1 and adjust with barium carbonate in the tank, not acid, when sulphate creeps.
Equipment side, set yourself up a small titration bench next to the line:
- One bottle of each standard, marked with prep date. Old thiosulphate lies.
- A log sheet, bath temp and reading together. The trend beats the number.
- Hex chrome PPE at the bench, gloves and eye protection, no exceptions.
- Same person does it daily where you can, technique matters more than people admit.
We put these little bench setups on planting lines all the time and the bath discipline improves within a month, simply because the number is in front of the operator instead of in a lab report nobody reads.