Electropolishing of SS.


(2000)

Hello, We are facing problem of white patches inside 1" Dia tubes ,3 mtr long which are being Electropolished by us.we immerse the tubes vertically in the bath.What are the cause? What are the remedies for removing the patches? Please suggest or guide us. Thanks, Mahesh.

Mahesh Raja
- mumbai,maharashtra,India


(2000)

Electropolishing requires high current density and fresh solution. It may be possible to electropolish this item with auxiliary cathodes and good solution changeover. But if you are just putting them into an electropolishing tank like any other work and are expecting the insides to polish up, then I think your expectations are probably unrealistic. Good luck.

Ted Mooney, finishing.com Teds signature
Ted Mooney, P.E. RET
finishing.com
Pine Beach, New Jersey


(2000)

The white patches appearing on the ID of your tubes could be a residue from your electrolyte. Insure that when you remove the tubes after processing from your tank, that the current is OFF and check your washing procedures giving particular attention to the internal surfaces.

Joel Levinsohn
Joel Levinsohn
- Sydney, Australia



This public forum has 60,000 threads. If you have a question in mind which seems off topic to this thread, you might prefer to Search the Site

ADD a Q or A to THIS thread START a NEW THREADView This Week's HOT TOPICS

Disclaimer: It's not possible to diagnose a finishing problem or the hazards of an operation via these pages. All information presented is for general reference and does not represent a professional opinion nor the policy of an author's employer. The internet is largely anonymous & unvetted; some names may be fictitious and some recommendations may be deliberately harmful.

  If you need a product/service, please check these Directories:

JobshopsCapital Equip. & Install'nChemicals & Consumables Consult'g, Train'g, SoftwareEnvironmental ComplianceTesting Svcs. & Devices


©1995-2017 finishing.com     -    Privacy Policy
How Google uses data when you visit this site.