PAINT RECIPE




I am looking for oil-based paint recipes or water-based paint recipes. Any recipes would be nice. I am doing a chemistry project and I need recipes to make paints if anyone can help me out I would highly appreciate it.

Thanks,

Kathleen
- Fulton, New York, USA
2003



2003

Here is a formulation from a course I took years ago.

Alkyd Gloss
11-064 Beckosol 150 g
Kadox 515 Zinc oxide 3.0 g
Titanox RA-45 300 g
Thixatrol ST 7.0 g High speed dispersed to a temperature of 52°C

Hegman >6
11-064 Beckosol 516 g
mineral spirits on eBay or Amazon [affil link] 170 g
6% Cobalt Naphthelate 3.3 g
24% Lead Naphthelate 50 g
4% Calcium Naphthelate 10 g
Exkin #2 1.0 g

Good luck.

Ronald Zeeman
- Brampton, ON, Canada


Sorry! Finishing.com is temporarily Read-Only.
Ted Mooney is retiring but I have several offers to take it over.
We're working hard to make sure we find it the best new home.





Disclaimer: It's not possible to fully diagnose a finishing problem or the hazards of an operation via these pages. All information presented is for general reference and does not represent a professional opinion nor the policy of an author's employer. The internet is largely anonymous & unvetted; some names may be fictitious and some recommendations might be harmful.

If you are seeking a product or service related to metal finishing, please check these Directories:

Finishing
Jobshops
Capital
Equipment
Chemicals &
Consumables
Consult'g,
& Software


About/Contact  -  Privacy Policy  -  ©1995-2026 finishing.com, Pine Beach, New Jersey, USA  -  about "affil links"