Copper/Aluminum interaction and galvanic/hydrolysis problems



Galvanic corrosion can occur if two different metals contact each other. The 3 things necessary for galvanic corrosion are:
    • Different metals or conditions such that one is more 'noble' than the other (copper is MUCH more noble than aluminum)
    • A conductive liquid path between them
    • A metallic connection allowing electrons to flow between them.
     Still, not all corrosion is galvanic corrosion; even standalone metals can rust or tarnish.

Q. Hello
I a DYI Person especially with my boat servicing and maintenance.
Recently I installed a new diesel fuel pick up in one tank.
I made the fuel pick up pipe out of 1/2" copper pipe approx. 12 inches in length
I had a suitable flange which is welded to the pipe with a brass hose connector. I have sealed off any metal connection with gasket material
My concern after doing this I was wondering if I may have a problem as the tanks are aluminium and really do not wish to have any corrosion issues ?

PT Taylor
- Auckland New Zealand
February 16, 2022


A. Hi PT. The bad news is that aluminum and copper are very highly incompatible galvanically.
But the good news is that you need both a conductive liquid path and a conductive metallic path to enable galvanic corrosion and you may have not even have either. Diesel fluid is not water and is quite non-conductive, and your gasket material seems to mean no metallic connection either (assuming there are no metal bolts through the gaskets holding the parts together).

Luck & Regards,

ted_yosem
Ted Mooney, P.E. RET
Striving to live Aloha

finishing.com - Pine Beach, New Jersey

Need quick confidential answers? $25
Need project assistance? $100/hr.


A. I have seen deterioration in exterior locations where light gauge sheet metal such as copper and galvanized are not physically connected and separated by six inches to several feet in a wall condition where rain water runs over them vertically and substantial corrosion occurs.

Gary Weaver
Forensic Building Enclosure Consultant - Irvine, California
December 11, 2024


thumbs up sign Thanks for the important warning, Gary!

I wonder whether, when you've seen this, the copper has been physically above the galvanizing? I've seen green copper stains run down onto stuff, and these copper salts on galvanized can certainly cause rapid galvanic corrosion. Similarly, copper dust from brake pads is often seen to cause pitting in aluminum wheels, and copper dust from overhead railway power feeds is seen to corrode aluminum benches and electrical panels.

I suspect that the reaction isn't between the two sheets, but between the copper salt or dust and the less noble metal it has landed on?

Luck & Regards,

ted_yosem
Ted Mooney, P.E. RET
Striving to live Aloha

finishing.com - Pine Beach, New Jersey

Need quick confidential answers? $25
Need project assistance? $100/hr.




Q. Someone on the net suggested dropping a short length of copper tubing into my pool skimmer basket to control algae. I'm pleased to report that it works. However, I also have a pool heater with an aluminum core. I'm concerned that the aluminum will be corroded because of the copper interaction through the water. Is this a concern?

PAUL E SIMPSON
Retiree - Meansville, Georgia USA
May 25, 2025


A. Hi Paul.

Metal-to-metal contact is necessary for galvanic corrosion, but the fact that the algae is being deterred tells us that the water has copper in it, so you have copper ions touching the aluminum.

Still, I suspect that the level of copper in the water -- only parts per million -- is so low that serious galvanic corrosion of the filter is highly unlikely.

Luck & Regards,

ted_yosem
Ted Mooney, P.E. RET
Striving to live Aloha

finishing.com - Pine Beach, New Jersey

Need quick confidential answers? $25
Need project assistance? $100/hr.




⇩ Similar, related, Q&As -- oldest first ⇩



Q. I am designing a cooling element to be used in a closed circuit fluid filled electrical component cooler. The heat exchanger and part of the cooling element are copper, and to save weight and price, part of the cooling element is aluminum. The pump may or may not also contain aluminum parts. I am aware of the galvanic corrosion problems of this combination of metals, both in theory and in first hand experience. My main two problems with this situation are 1.) Precipitation of oxides out of the cooling fluid which would clog the system. and 2.) Consumption of the aluminum parts that may cause leakage. I would sincerely appreciate any suggestions to prevent these two occurrences. These are the options I have examined so far:

1.) Place a sacrificial anode in the system to protect the aluminum. To my knowledge this would be ineffective due to the precipitation problem.

2.) Coat the aluminum parts with a thin polymer to protect it. What about scratches, durability?

3.) Add an inhibitor to the coolant. I think this would be a temporary solution that would have to be monitored and refreshed cyclically.

Paul Seabury
- College Station, Texas
2001


A. Answer number 3 may well be temporary, but it is certainly widely practiced in everything from automobile radiators to industrial boilers and cooling towers.

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha

finishing.com - Pine Beach, New Jersey

Need quick confidential answers? $25
Need project assistance? $100/hr.


A. Paul:

There might be a third alternative. Have you considered designing your system to operate with oil, is it feasible? Many oils are almost dielectric, so galvanic corrosion would not take place or would be reduced to minimum. Hasta la vista.

Guillermo Marrufo
Monterrey, NL, Mexico


thumbs up sign I did some more research, and came up with the polymer coatings Nycote [adv: Nycote on eBay] and Topcoat. These seem like longer lasting solutions, but I would like to hear of anyone else's experiences with them. I would also like some availability information if anyone has it as I have initially had a really tough time finding suppliers for Nycote in the US (much less pricing). Thank you for your response Mr. Mooney. I still have reservations about adding an inhibitor though, as the product design calls for a solution to be more or less permanent.

Thanks again,

Paul Seabury
- College Statio, Texas




Q. I am designing a water cooling system, with a small copper heat exchanger and a large aluminum radiator. Will there be a corrosion problem between the two different metals after a few years of continuous use, water temperature will be about 50C Anodized aluminum would be better but this is for a one off project and I was hoping to avoid any special finishes?

Mark Cumper
Designer - Antwerpen, Belgium
2003


A. I don't exactly understand the description, Mark. But it sounds like trouble. Aluminum is a very active metal and copper a quite noble one. If both materials touch the same fluid, allowing an ionic path, and there is a metallic path as well, galvanic corrosion seems pretty likely.

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha

finishing.com - Pine Beach, New Jersey

Need quick confidential answers? $25
Need project assistance? $100/hr.



Q. If the copper and aluminium are not connected electrically, except by the water does this improve matters ? Does earthing everything help, or make matters worse by preventing an equilibrium from ever being established ? I thought that if the area of copper was much smaller than the area of Aluminium, then it would be OK.

Mark Cumper
- Antwerpen, Belgium
2003


A. Having a small surface area of the more noble metal certainly helps, but I don't think it makes things "okay". However, if the metals are not connected except by the water, I don't believe that galvanic corrosion is possible because you have no metallic path for electron travel.

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha

finishing.com - Pine Beach, New Jersey

Need quick confidential answers? $25
Need project assistance? $100/hr.


thumbs up sign So insulating the copper is all I need to do. Great news.

Thank you for your help.

Mark Cumper
- Antwerpen, Belgium


A. I would say analyze your water before proceeding. Aluminum has an excellent oxide layer. If the level of chloride & sulfur & copper is low in water, aluminum can be used. Pitting is the issue in aluminum. Copper does better than aluminum for atmospheric corrosion but it is quite susceptible at various pH levels. Overall aluminum shows lower corrosion rates. pH for aluminum use is between 3.8 to 8.

Small copper to large aluminum sounds like a good plan as far as the area for galvanic goes.

Kam Dianatkhah
- Dallas, Texas






Q. I have a client that has a Mansard style roof made of copper. He would like a decorative fence on the top flat portion of the roof. We are thinking of using an aluminum powder coated or painted railing. The railing will never touch the copper. Will the rain water that hits the aluminum cause corrosion on the copper? Or will it affect the patina finish that is on the copper roof?

Thanks,

Darren Ratzow
Home Builder - Oconomowoc, Wisconsin, USA
2004


A. Galvanic corrosion is possible if there is a metallic path (through screws). If there is not a metallic path, galvanic corrosion cannot occur. Even if it did, copper is the noble metal and aluminum is the active metal, so it is the aluminum that would corrode. Patinas, however, are tricky things; so I personally would not promise no effect on the patina if there is in fact a metallic path.

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha

finishing.com - Pine Beach, New Jersey

Need quick confidential answers? $25
Need project assistance? $100/hr.






Q. Hi, we are currently using a thermally clad printed circuit board with aluminum base that has many high current LEDS. The aluminum underside of assembly is coated in Dow Corning 340 non curing paste and bolted to an anodized Aluminum extrusion through which water is circulated @20 °C. We have the option of replacing the aluminum base of thermally clad board with a copper base with improved thermal conductivity. However will I have aluminum-copper interaction problems when bolting the new copper base to aluminum extrusion.
Will the aluminum suffer corrosion?

Pauric Hennessy
lighting - Ireland
2005


A. Any path for electricity and transfer of atoms (ions) means aluminum will be sacrificed by copper. Such a case would happen with humidity.

Guillermo Marrufo
Monterrey, NL, Mexico


A. Copper is PLUS 0.34 volts OVER Hydrogen. Aluminum is negative 1.7 volts UNDER Hydrogen, that is 2.04 apart with Copper the anode, therefore copper would be sacrificed to the aluminum. However, if chlorides from salt air is around, then the aluminum will also be corroded. Properly sealed, preferable dichromate sealed, aluminum is non conductive and hence zero with respect to hydrogen.

robert probert
Robert H Probert
Robert H Probert Technical Services
supporting advertiser
Garner, North Carolina
probertbanner


A. Robert, I believe that, while your numbers might be correct, your conclusions are the reverse of what is correct.

Is not Guillermo's conclusion correct, and the aluminium will corrode while the copper will not corrode?

Bill Reynolds
Bill Reynolds [deceased]
consultant metallurgist - Ballarat, Victoria, Australia
We sadly relate the news that Bill passed away on Jan. 29, 2010.



The aluminum is "anodic protected". The Anode "gives", the cathode "receives".

When you anodize 2024 the copper plates out (but may not bond), onto the cathode (aluminum or lead or stainless steel).

In this case the copper dissolves away from the higher potential and tries to plate on (and may not bond) to the lower potential.

robert probert
Robert H Probert
Robert H Probert Technical Services
supporting advertiser
Garner, North Carolina
probertbanner


I must continue to disagree, Robert. You're trying to turn the whole electrochemical series on its head by saying that the more noble metal corrodes while the less noble metal gives protection.

The reactions that may occur in anodising, where a large voltage/current runs through an electrolyte between two dissimilar metals that are not otherwise joined, are not relevant to the case described by Pauric Hennessy. He proposes simply clamping aluminium and copper together and wonders if there will be corrosion of one or the other. As Guillermo says, in the presence of humidity, the aluminium will corrode, as per the electrochemical series.

Will somebody else please buy into this discussion? Am I missing something that Robert sees, or is Robert seeing something that isn't actually there?

Bill Reynolds
Bill Reynolds [deceased]
consultant metallurgist - Ballarat, Victoria, Australia
We sadly relate the news that Bill passed away on Jan. 29, 2010.




Aluminium is often used to protect copper water pipes from pitting. The aluminium is referred to as a sacrificial anode, as it will dissolve under these conditions. That makes the aluminium anodic and the copper cathodic. However, aluminium is usually covered in a protective and tenacious metal oxide that significantly shifts the oxidation potential of the "aluminium"; actually the potential in this case will be that of the aluminium oxide. Exactly how the aluminium-copper system will corrode will depend on the environment it is in. If the chemical environment promotes failure of the aluminium oxide layer, then the aluminium will corrode, if it does not, the copper MAY corrode.

trevor crichton
Trevor Crichton
R&D practical scientist
Chesham, Bucks, UK


? Now, I'm more confused. Is it correct that aluminum oxide is dielectric or non conductive? If so, how could it have a position in the galvanic series? The only possibility I see is that there are pores in the oxide layer produced by anodizing an aluminum surface. Someone please comment in this direction.

Guillermo Marrufo
Monterrey, NL, Mexico
2005


thumbs up sign Ever since Mr. Probert started noting here that anodized aluminum is non conductive (which goes back a couple of years now), and which was something I always knew but hadn't really thought through, I've noticed the many outdoor applications of anodized aluminum fastened with stainless steel bolts, or u-bolted to galvanized metal, etc. And my observation has been that this seems to cause little to no galvanic corrosion problem in most cases. If the anodized coating were broken where it meets with the other metal, I guess it would be a problem. But if the anodized coating is broken elsewhere than at the connection, there still would be no metallic conductive path and apparently no galvanic corrosion. So it's good theory and born out by experience.

But as for this particular question, Mssrs. Reynolds and Crichton must surely be right: aluminum is the base metal that corrodes and copper is the noble metal that is protected.

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha

finishing.com - Pine Beach, New Jersey

Need quick confidential answers? $25
Need project assistance? $100/hr.


A. Gentlemen:
From an everyday application and interaction of metals standpoint, we build MRI room [Faraday Cages.]
The most common observation has been that in the absence of special finishes, in an intentionally conductive application, the copper will always corrode the aluminum. To prevent/delay the reaction, we normally sandwich stainless components depending on the application to safe guard the aluminum leaving it now solely exposed to moisture effects.
So in magnetic fields and ground isolated rooms, the metal nobility relationship seems to always rule the day.
I hope this helps a little to clarify which metal would otherwise always corrode on contact.

Luis G. Botero
- Riverside, California, USA
November 25, 2008


A. Aluminum fins are pressure bonded to copper tubes in cooling coils. A manufacturer recently disabused me of the notion that a little bit of insulating goo was attached to the aluminum fins before the tube was expanded into a tight fit with the aluminum fin.
Water will run off of the dehumidifying aluminum and copper evaporator, and, if the identically configured coil is condensing in the rain, the entire coils will get wet, yet they will last almost indefinitely.
However if one sprays either coil with tap water, as is often done to bring down the condenser temperature on a hot day, or on the evaporator for humidification, the aluminum will rot away or oxidize into a brittle non conducting useless wafer within a year.
I don't get it.

Jack Hunt
HVAC Consulting - Los Gatos, California, USA
July 28, 2010


A. I have worked in electrical distribution for many years and I can definitely say that in bi-metallic joints between copper and aluminium, the aluminium corrodes away and the copper stays intact.

Thunder Lightning
- UK
June 12, 2012


A. I have inspected over 70 newer wood decks attached to aluminum sided homes which used ACQ treated wood in the deck with the results being the dissolution of the aluminum siding into fine lace. In areas of high rain water splashing the aluminum siding is proportionately dissolved.

Terry Ethridge
Home Inspector - Kingston, Ontario, Canada
July 3, 2012



thumbs up sign Very interesting, Jack. Apparently rainwater, which is distilled, is sufficiently non-conductive that there is no significant galvanic action. Galvanic activity requires two metals of different potential (copper and aluminum - check), a metallic connection between them (check), and a conductive fluid in contact with both of them (tap water: check; rainwater: no check?).

Thunder: Your parents were quite the jokesters. I suppose your sister's name is Heat  🙂

Hi Terry. Thanks. Speaking as a homeowner, not as a professional, ACQ is murderous. I used electrogalvanized (zinc plated) deck screws on some mixed CCA and ACQ for a deck repair and every one in the ACQ was totally gone (rusted completely through) in less than one year. The earlier types of pressure treated wood like CCA may have been more dangerous in some ways, but ACQ is way, way more corrosive to anything it touches than CCA was, and I would certainly expect that this greatly increased amount of copper leaching out is quite bad for some life forms.

Regards,

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha

finishing.com - Pine Beach, New Jersey

Need quick confidential answers? $25
Need project assistance? $100/hr.






Q. Our shop fabricates and repairs current carrying arms for electric arc furnaces. We are having trouble with one particular set of arms that are built from 6061-T6 aluminum. The front contact surface of these arms is a 1/2" thick c101 copper plate that is explosion bonded to the aluminum. The arm body appears to be experiencing severe galvanic corrosion at the point where the copper and aluminum meet.

56063

We have tried using a ceramic coating on the arms, and it helps slightly, but doesn't hold up to the harsh environment these arms are exposed to. We also recently purchased a new set of explosion bonded front plates with a .015" thick niobium interlayer between the copper and the aluminum to experiment with. We are looking for some input to make sure we are going in the right direction, and possibly some suggestions for preventing the corrosion.

Thanks,

James Finley
Service Technician - Huntington, West Virginia, USA
November 2, 2010




Q. We have a big problem with hydrogen gas released in the radiators made of aluminium.
(some parts of wall hung boilers are made of copper.)
Some hydrogen gas is released inside the radiators and they can't get warm completely.
Can anybody say is there a way to stop this reaction, at least not to release the hydrogen gas?

Is there something to add to the water to stop this?

Sarbast parvizy
hydronic heating technician - sanandaj, kurdistan, iran
February 26, 2013






Q. Hi all! great forum!! congrats!!

I would like to discuss about a possible project I am trying to design.

I would like to use aluminum tubing (probably annealed 3003 series) to circulate liquid (water based with some anti-freeze, similar to car engines coolant) to gather energy (heat) toward an open loop liquid reserve.

I am afraid of the longevity of the system because of possible corrosion inside the aluminum tubings (probably ~0.5" ID)

Is it very dangerous if some copper components are installed somewhere in the loop (without direct contact to aluminum piping of course)?
Could be in the form of a valve or a few connections. Would represent a very small % of the total area

Also, if some copper pipes would be used as exchanger coil within the liquid reserve? same problems?

Then lastly, is there any way to setup sacrificial metal in the reserve and some environmentally friendly additives/inhibitors that you would recommend ?

Most car engines feature parts in aluminum and steel, and some older cars even had radiators and heater cores done in copper and I don't recall to notice a problem with galv corrosion on the alum parts or it was very small even after 10-20 years usage with coolant.

Thanks all for your time!

John Poirier
designer, interested - Montreal, Quebec, Canada
March 21, 2013


A. Hi John. You cannot (as far as I know) have galvanic corrosion without a metallic connection between the two metals. Yes, the corrosion inhibitors in automobile antifreeze are quite effective  🙂

It is possible to use magnesium anodes as sacrificial anodes if desired -- they are used in home water heaters and on fresh water boats.

Luck & Regards,

ted_yosem
Ted Mooney, P.E. RET
Striving to live Aloha

finishing.com - Pine Beach, New Jersey

Need quick confidential answers? $25
Need project assistance? $100/hr.


Sorry! Finishing.com is temporarily Read-Only.
Ted Mooney is retiring but I have several offers to take it over.
We're working hard to make sure we find it the best new home.





Disclaimer: It's not possible to fully diagnose a finishing problem or the hazards of an operation via these pages. All information presented is for general reference and does not represent a professional opinion nor the policy of an author's employer. The internet is largely anonymous & unvetted; some names may be fictitious and some recommendations might be harmful.

If you are seeking a product or service related to metal finishing, please check these Directories:

Finishing
Jobshops
Capital
Equipment
Chemicals &
Consumables
Consult'g,
& Software


About/Contact  -  Privacy Policy  -  ©1995-2026 finishing.com, Pine Beach, New Jersey, USA  -  about "affil links"