I'm looking for a source or vendor for plating platinum on some small to medium sized titanium parts. The platinum is required for corrosion resistance not appearance. Good adhesion is critical. Any suggestions are welcome.

Bob Batz
- Rochester NY USA


.

Dear Bob

Plating titanium with platinum is usually done in melt of salts (KCN and K2Pt(CN)4), using the titanium as cathode and platinum as an anode. There are very few firms that use this process for making anodes e.g. for chrome baths. A firm that uses this process is Degussa in Schwbisch Gm¸nd Germany, but I do not know if they want to plate special parts like yours. You can ask also suppliers for platinum plated titanium anodes for chrome baths where they plate them and maybe you find someone there who can plate your parts,too.

Good luck
Marcus

Marcus Hahn
- Sachseln, Switzerland


.

Plating on to metals like titanium, zirconium, uranium, etc, that are very oxygen active is often done with ion plating, a PVD process. In some cases a "strike" is put on by ion plating and the coating built up by electroplating.

Donald M. Mattox
Society of Vacuum Coaters
Albuquerque, NM
 
Ed. note:
            Mr. Mattox is
            the author of --


.

Bob,

Electroless platinum plating technology which might be applicable to your particular situation. A nickel strike may be required in order to get good adhesion onto the substrate. Good luck with your search.

Jeff Venarsky
- Jerseyville, Illinois


+

Dear Mr.Bob Batz,

We electrodeposit platinum on titanium with plating thickness up to 10 micron with a good adhesion properties.

H.H.Madhani
plating shop - Pune, MH, India


Dear Reader: please choose what you want to do.

I want to post a question or inquiry of my own.
 
I want to answer this question publicly
 
I am a supporting advertiser and want to reach the inquirer privately.





     

 Save This Page (why?)    -    Home    -    ©1995-2008 finishing.com