What is Kesternich Test? SO2 Sulfur Dioxide Corrosion Test? Need to pass 72 hours





RFQ: I'm looking for a source for Kesternich testing per DIN 50018. Does anybody have a reliable lab they can refer me to?

Christa Shirey
- Sylvania, Ohio
1999

Ed. note: This RFQ is outdated, but technical replies are welcome, and readers are encouraged to post their own RFQs. But no public commercial suggestions please ( huh? why?).



A. Hey Christa,

Kesternich: German scientist who developed the Kesternich Cabinet and test method used for acid rain simulation (DIN 50018).

U.S. INTEC, Inc. tests their Roofing and Building Fasteners using the Kesternich test. Talk to the tech people at U.S. INTEC, Inc. Port Arthur, Texas.

Hope this helps,

Fred Mueller, CEF
- Royersford, Pennsylvania
1999




Q. I work for a coatings company that has designed a coating for electrical metallic tubing. One of the tests that the coating must pass is corrosion resistance in a moist carbon dioxide/sulfur dioxide-air environment. I have never heard of this test. Has anybody else? Does anybody know who performs this test?

Michael A. Koons
- Berea, Ohio USA
2000


A. Michael - I have a copy of the test I believe you are referencing. If you will give me your fax number,I'd be happy to send it to you. It includes CO2/SO2.

Cynthia L. Meade
- Sylvania, Ohio, USA
2000


thumbs up sign I would like to get a copy about the corrosion test of metals with CO2 and SO2.

Thanks!

Joe Shi
Visteon - Dearborn, Michigan, USA
2001




Q. I am working with a coat of copper/nickel, a thickness of 10 microns and 3 microns, without passivation. I know that Kesternich test is very aggressive for such finish but I have read that I can make this test with this finish using only 20 ml of SO2, with this quantity I can see results. I normally work with a bottle of SO2 gas, introducing 0.2 L or 2 L in the Kesternich chamber, so I can't control with this bottle 20 ml that is necessary for the test with a Copper/nickel coat. I read that it's possible to produce SO2 inside the chamber without gas, in another form. Is it possible?, How can I do it? Which are the compounds I need and the quantities for 20 ml?

Sonia Egiguren Aristizabal
- San Sebastian, Spain
2002




Q. I would like to know if there are more standards for this kind of test and for artificial atmosphere Salt spray tests.

Ana Sofia Torres
metallurgy - Portugal
2005


A. The specifications we use most often are DIN 50018, ASTM G87, ASTM G85 Annex A4, and ISO 3231. You can purchase the DIN specification at www.global.ihs.com, the ASTM specifications at www.astm.org, and the ISO specification at www.iso.org. They should be available for download.

Christa Lammers
-Sylvania, Ohio, USA
2005



2005

For the SO2 test you have: IEC 60068-2-42 Kc

For the salt spray test you have various methods given in IEC 60068-2-52 Kb

or

IEC 60068-2-11 Ka

Alexandra Lese
- Nurnberg, Germany


Ed. note: For your convenience (and for our potential commissions), we've also linked to a source that offers specs from all these standards bodies.



Multiple threads merged: please forgive chronology errors and repetition  🙂



2005

Q. I am working in corrosion testing of Mullite coatings. I wanted to know what is Kesternich test and who can do some testing of my sample.

Soobhankar Pati
Boston University - Boston, Massachusetts

Ed. note: This RFQ is outdated, but technical replies are welcome, and readers are encouraged to post their own RFQs. But no public commercial suggestions please ( huh? why?).


A. Hello Soobhankar.
Kesternich testing is a common name for sulfur dioxide testing. There are several test methods available. DIN 50018, ISO 3231, and ASTM G87 are some of the more common methods.

Christa Lammers
-Sylvania, Ohio, USA
2005




Q. I am running Sulfur Dioxide Salt Fog Tests in accordance with ASTM G85 -02 Annex 4. Continuous spray with SO2 injection for 1 hour every 6 hours. The pH of the collections should be 2.5-3.2. My pH is consistently 2.0-2.3. I am injecting gas at the rate of 1cc/min/ft3 of chamber volume. The flow meter is calibrated for SO2 so I am confident the flow rate is correct. The chamber was purchased new within the last year. My pH probe is calibrated daily with ph 4,7, and 10 buffer solutions. After calibration I check the ph of a 1.68 buffer solution and range 1.62 to 1.68. Any suggestions why my ph is low.

Gary Hyland
testing laboratory - Bohemia, New York
2006



A. Hello -
Are you metering SO2 based on the nominal cabinet volume, that is, the usable testing space that does not include the cover or other volume not a part of corrosion testing? There is often 50% larger volume to take into account when injecting gas since it diffuses throughout the cabinet regardless of how certain test methods define working volume. But, it is certainly a puzzle why the pH is low. How old is the salt solution - has it had a chance to sit around and drop its pH below 6.5? Perhaps buffering the pH of the salt solution to the high end of neutral - closer to a pH of 7.2 - will help.

Harold D. Hilton
salt spray cabinet mfgr. - Chicago, Illinois, USA
2006




Need chrome plating to survive 72-hours of SO2 corrosion testing

Q. We want to develop chrome plating which can withstand SO2 corrosion testing for 72 hours

Suvidh Mehta
- Jamnagar india
January 1, 2020



January 2020

A. Hi Suvidh. My understanding is that nickel-chrome plating should normally be able to survive three 24-hour Kesternich cycles (72 hours total).

Please introduce yourself and your situation: Are you talking about hard chrome plating (engineering chrome) or decorative nickel-chrome or copper-nickel-chrome plating? Are you a process supplier who will be offering this process for sale to plating shops, or are you a plating shop, or are you a product manufacturer who wants to get your parts plated?

Are your parts currently failing this test? If so, what is the plating specification, and what test specification are you following? Pulse plating of chrome is reputed to decrease porosity and increase Kesternich resistance. Thanks.

Regards,

ted_yosem
Ted Mooney, P.E. RET
Striving to live Aloha

finishing.com - Pine Beach, New Jersey

Need quick confidential answers? $25
Need project assistance? $100/hr.



January 2, 2020

Q. MY NAME IS SUVIDH MEHTA LOOKING FOR DEVELOPMENT IN FAUCET MANUFACTURING COMPANY IN INDIA.
WE ARE DOING DECORATIVE CHROME ON FAUCET PARTS
WE HAVE OUR OWN ELECTROPLATING UNIT
ONE OF OUR CUSTOMERS ASK FOR SO2 CORROSION TEST FOR 24 HOURS 3 CYCLE BUT OUR SAMPLE FAILS
WE ARE DOING COPPER 10 MICRON
NICKEL 10 - 25 MICRON
CHROME - 0.20 MICRON MINIMUM
WE OBSERVED CORROSION AFTER 24 HOURS AND SOMETIMES AFTER 48 HOURS

SUVIHD MEHTA [returning]
SYSTAMET INDIA PVT LTD - jamnagar, India



A. Thanks for the follow-up Suvidh. There are three possibilities here:
-- The first is that the overall design of your process is not adequate to deliver three successful cycles, and you will have to upgrade your whole nickel and chrome plating process.
-- The second possibility is that something more minor is wrong and requires adjustment.
-- The third is that the test is not being conducted correctly.

The Kesternich/SO2 test is not particularly common, and I think that makes it hard to find good data for comparison, as well as increasing the likelihood that something is not right in the testing procedure.
So I think something which might be very helpful in making that determination would be the results of some other accelerated corrosion test. Are you doing, or have you recently done, any other corrosion testing like CASS or Corrodkote on the parts?

Regards,

ted_yosem
Ted Mooney, P.E. RET
Striving to live Aloha

finishing.com - Pine Beach, New Jersey

Need quick confidential answers? $25
Need project assistance? $100/hr.
January 2020



Q. Can you please assist in setting our nickel and chrome plating line according to requirement.

SUVIHD MEHTA [returning]
SYSTAMET INDIA PVT LTD - jamnagar, India
January 4, 2020


Sorry! Finishing.com is temporarily Read-Only.
Ted Mooney is retiring but I have several offers to take it over.
We're working hard to make sure we find it the best new home.





Disclaimer: It's not possible to fully diagnose a finishing problem or the hazards of an operation via these pages. All information presented is for general reference and does not represent a professional opinion nor the policy of an author's employer. The internet is largely anonymous & unvetted; some names may be fictitious and some recommendations might be harmful.

If you are seeking a product or service related to metal finishing, please check these Directories:

Finishing
Jobshops
Capital
Equipment
Chemicals &
Consumables
Consult'g,
& Software


About/Contact  -  Privacy Policy  -  ©1995-2026 finishing.com, Pine Beach, New Jersey, USA  -  about "affil links"