Interference of phosphating layer with press fit [India] 

March 27, 2006

I have an application where a phosphated sintered female part namely Hub (density 6.5~7.0 g/cc) is press fit with a steel shaft. The design interference is 0.060mm to 0.100mm (0.0024" -0.0039"). Recently I had lot of failures where hubs slipped off from the press fit under working condition. We have specified phosphating layer in the bore to an extent of 0.005 to 0.012 mm (0.00019" - 0.00047"). My query is whether the presence of such phosphated layer in the interference will weaken the joint or not?


G. MURALIDHARAN

Auto ancillary - Chennai, Tamilnadu, India


March 29, 2006

Most likely the cause may be an over etch during the pre-cleaning or an over exposure to the phosphating solution of the parts.

Guillermo Marrufo
Monterrey, NL, Mexico


March 30, 2006

My thought would be that the interference fit is crushing the phosphate to a fine powder which can work out and also act as a lubricant.

James Watts
- FL


April 18, 2006

Thanks for the responses. I am glad that I could move a step or two forward with these inputs.

G.Muralidharan
- Chennai, Tamilnadu, India

"Phosphating of Metals" by Rausch is also available from --

this link at
Abebooks.com (USA)

or

this link at
AbeBooks.co.uk (U.K.)


Dear Reader: please choose what you want to do--

I want to answer or follow-up on this subject publicly (in non-commercial fashion).
 
My company is a supporting advertiser at finishing.com and we want the contact information to reach the inquirer privately.
 
I want to post a new question or inquiry of my own on a different subject.
 





     

 Save This Page (why?)    -    Home    -    ©1995-2008 finishing.com