Letter 30042
Specs for bright dipping copper and brass
[Ohio]
++++
Are there any specifications out there for bright dipping copper
and brass?
Bob R
[last name deleted for privacy due to age of posting]
plating shop - Elyria, Ohio
+++++
Here we do Bright dipping of copper Terminals which are used in
Automotive batteries.
The Process Flow is as below:
1. Cleaning : By means of Kerosene and Saw Dust
2. Rinse : Rinse the material by means of Raw Water
3. Solution Make Up: Ratio of 4:1:1 (4 Parts of DM Water : 1 Part of
Nitric acid & 1 Part of Sulphuric acid all are commercial grade
chemicals)Dip in the same for few seconds as the copper will melt in
the solution its just a surfce preperation for the adhesion of
PASSIVATION.
4: Rinse : Raw water Rinse Twice
5: Passivation : Yellow color as per u r requirement
6: Rinse : Raw Water Dipping once
7: Dryiing : any type of Dryer can be used
Regards
T.Dinakaran
T.DINAKARAN
- Chennai,Tamilnadu .INDIA
Dear Reader: please choose what you want to do--
- I want to answer or follow-up on this subject
publicly (in non-commercial
fashion).
-
- My company is a supporting advertiser at
finishing.com and we want the contact information to reach
the inquirer privately.
-
- I want to post a new
question or inquiry of my own on
a different subject.
-
 |