  Thread 21/11

Solutions to Problems with cleaning brazed Copper product




I am in the process of manufacturing a brazed copper product but have not found a quick way to get it back to its bright finish. Help!

James Caffrey
- Bozeman MT
1998
publicly reply to James Caffrey


You need to apply proper chemistry, and I don't know if you have the in-house capability or if you need to find a jobshop. But bright-dipping of copper is a fairly common procedure for jobshops. You need an acid and an oxidizer. Perhaps the most popular today is the sulfuric-peroxide bright dip offered as a proprietary by Electrochemicals and perhaps others; but there are also nitruc acid based bright dips for copper.

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
1998
publicly reply to Ted Mooney

Can you provide sources for the nitric acid based bright dips for copper? I would like more info on that process. Respectfully,

Kenneth Waldrop
- Austin, Texas
1999
publicly reply to Kenneth Waldrop


2001

James,

the best luck I've had with copper alloy bright-dipping solutions is: 60 v/v% sulfuric acid, 66 baumé, 20 v/v% nitric acid, 42 baumé, 2-6 milliliters per liter hydrochloric acid (I used Printed Circuit Grade, 22 baumé), and de-ionized water, 20 v/v%. Add the DI first, then sulfuric, nitric, and hydrochloric.

Preparation of this solution liberates marked heat, so wear your PPE!

Blend the solution gently, allow it to cool, then run some scrap copper parts through it to generate kinetic ion activity before running your good alloys. Dipping the parts in a solution of 50% hydrochloric acid prior to the bright dip is recommended.

This solution works on manganese bronze, commercial brass, neat copper, you name it! .

randy fowler
Randall Fowler - Fowler Industrial Plating, LLC
Cleveland, Tennessee, USA
publicly reply to Randall Fowler



(No "dead threads" here! If this page isn't currently on the Hotline your Q, A, or Comment will restore it)

Q, A, or Comment on THIS thread -or- Start a NEW Thread


Disclaimer: It's not possible to fully diagnose a finishing problem or the hazards of an operation via these pages. All information presented is for general reference and does not represent a professional opinion nor the policy of an author's employer. The internet is largely anonymous & unvetted; some names may be fictitious and some recommendations might be harmful.

If you are seeking a product or service related to metal finishing, please check these Directories:

Finishing
Jobshops
Capital
Equipment
Chemicals &
Consumables
Consult'g,
& Software


About/Contact  -  Privacy Policy  -  ©1995-2025 finishing.com, Pine Beach, New Jersey, USA  -  about "affil links"