Stainless steel 316L versus 904L




Q. I know stainless steel 316L is used in pharmaceutical and medical environments, I would like to know if stainless steel 904L can be used as a substitute and if it matches FDA and international standards the same as 316L does.


Rene Harmsen
- Amsterdam, The Netherlands
2002


A. 904L has greater amounts of chromium and nickel than the 316L grade. It is typically used in the chemical industry for severe corrosion environments i.e better resistance to pitting, SCC, IGC etc. In terms of matching international standards I am unsure as to why it would not. The only problem I see with this alloy is that it would be a great deal more expensive than a 316L grade stainless steel.

One thing to note is that the Molybdenum content in the 904L is around 1-2% in comparison to the 316L which is typically 2-3%. This may have an impact upon the pitting resistance of the 904L, but I guess an appropriate corrosion test would indicate this.

Matthew Hogan
- Melbourne, Australia
2002


A. Concerning Matthew's comment on pitting...

A useful parameter is the Pitting Resistance Equivalent Number (PREn), which is Cr% + 3.3 x Mo% + 16 x N%. The higher the value, the better the pitting resistance (the "N" in the formula is nitrogen, not a typing error for nickel).

Bill Reynolds
Bill Reynolds [deceased]
consultant metallurgist - Ballarat, Victoria, Australia
We sadly relate the news that Bill passed away on Jan. 29, 2010.

2002



Q. I know that 904L has a better corrosion resistance but what I need to know is whether or not 904L may be used in medical / pharmaceutical environments. I am concerned because of the 1-2 % copper that is part of the formula.

Thanks in advance.


Rene Harmsen
- Amsterdam, the Netherlands
2002


A. If the material doesn't corrode in the application, then the copper in the alloy, as well as the chromium, nickel, molybdenum, manganese, silicon and all the rest, will not be released to enter whatever liquid is in contact with the metal.

Notwithstanding, there may be some national statutory regulation that applies. Such regulations are often written by idiots and have no technical justification, and vary from country to country, but if they exist then unfortunately they have to be complied with.

Bill Reynolds
Bill Reynolds [deceased]
consultant metallurgist - Ballarat, Victoria, Australia
We sadly relate the news that Bill passed away on Jan. 29, 2010.

2002


Actually, the moly in 904L is 4-5% NOT 1-2%. It is more expensive than 316L and the 904L has been used in pharmaceutical applications in the past. The price is keeping it from seeing more widespread usage.

Daryl Coleman
- Lakeland, Florida
2007



My Respect to Late Mr. Bill. I am a Metallurgist and seeing this site for the first time.

Now, our body has fluid containing UREA as well as Chloride Ions. I have seen 316Mo grade used in Plant manufacturing UREA Grade Fertilizer. 904L has higher Mo ... so use it. But ensure that the Inclusion is never above 0.5 Thick and Thin as per ASTM E45 (type A, B, C and D)

Mr. S. H. Shah
- Ahmedabad, Gujarat, INDIA
June 17, 2010


Q. What are the advantages of using HASTELLOY instead of 904L, for sulfuric acid?

I am going to use 904L which is much cheaper, will it be suitable?

Efthimis Patsialos
sales - Athens
2007


Q. Dear Sir,

My customer is asking for 904L grade. Can I suggest him 316L according to the discussions in previous questions considering the cost involved in this?

Mahesh Durairaj
steel manufacturing - Chennai,Tamil Nadu, India
January 19, 2010




Q. Hello, I work in soda ash industry, Khewra.
I want to ask which is more corrosion resistant against chloride ions and more economical to use in our pipes: Should I go for 904L or 2205 (S31803)?
Note that there is no sulfuric acid flowing in the pipes.
Thanks,

Asif Ijaz
- Khewra, Pakistan
July 11, 2012



Q. SS316L Or SS904L -- Which material have more corrosion & erosion resistance. I am going to use this rotating equipment in heavy dust environment.

Chandar Gopal
- Tamilnadu, India
March 17, 2013


Sorry! Finishing.com is temporarily Read-Only.
Please maintain your bookmarks! Although Ted Mooney is retiring, finishing.com is not!
It will have a new owner/curator very shortly!



Disclaimer: It's not possible to fully diagnose a finishing problem or the hazards of an operation via these pages. All information presented is for general reference and does not represent a professional opinion nor the policy of an author's employer. The internet is largely anonymous & unvetted; some names may be fictitious and some recommendations might be harmful.

If you are seeking a product or service related to metal finishing, please check these Directories:

Finishing
Jobshops
Capital
Equipment
Chemicals &
Consumables
Consult'g,
& Software


About/Contact  -  Privacy Policy  -  ©1995-2026 finishing.com, Pine Beach, New Jersey, USA  -  about "affil links"