| Search our quarter-million Q&As |
Home of the finishing HOTLINE since 1989
-----Electropolishing or Chemical Polishing of Gold Q&A
Q. I'm looking for a way to etch and electropolish an approx. 70% gold, 30% platinum alloy. Please let me know if you have any suggestions or references I can look at.
Silvia Marinache1998
|
|
Q. I require the process and chemicals for electropolishing gold, 18-22 carat ornaments Please advice the availability of the same. Thanks - sharjah, U.A.E. 1998 Q. LOOKING FOR CHEMICALS FOR ELECTROPOLISHING OR CHEMICAL POLISHING OF GOLD JEWELRY. RAJA R.A.- AL-AHMADI KUWAIT 1998 Ed. note: This RFQ is outdated, but technical replies are welcome, and readers are encouraged to post their own RFQs. But no public commercial suggestions please ( huh? why?). |
A. I was looking for the same information - specifically information on all types of electropolishing. Perhaps not much help but there was a chemical company out there called Metal Coating Process Corp.. They gave a dissertation on electropolishing - If anyone knows about this, they seem to!
Hope this was helpful?
Hank Merkle1998
A. Hi. Yes, Metal Coating Process Corp. specializes in electropolishing equipment, chemistry, and training.
Regards,

Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
Need quick confidential answers? $25
Need project assistance? $100/hr.
Multiple threads merged: please forgive chronology errors and repetition 🙂
Q. I am seeking advice upon the conditions for electropolishing gold. Initial trials with a recipe using a mixture of ethylene glycol and HCl have shown that it is not trivial in practice to find the conditions for polishing without deep etching. I would be pleased to hear from anyone with practical experience of this system, about the details of their procedure.
Trevor RaymentCambridge University - Cambridge UK
1998
⇦ Tip: Readers like to learn from others' situations;
some readers skip abstract questions.
Q. REQUEST INFORMATION ON ELECTROPOLISHING OF GOLD ORNAMENTS, i.e. 22 carat or 18 carat. please advice
MUNIS M. MOTIWALAAL ASRIAH METAL COATING - SHARJAH,U.A.E.
1998
1999
A. Gold Electropolishing must be run for few seconds and at very high temperature.
- Operating conditions
- Temperature 70 °C
- Voltage 13 V minimum and it depends of the size of the pieces
- Time 15 - 30 SECONDS
- Voltage 13 V minimum and it depends of the size of the pieces
Tell me if the pieces you polish are produced by melting, or another method. And also the pretreatment you run before the electropolishing. Bye bye.
Giuseppe Pappi- A.G.E. di G. Pappi - Vicenza ( Italy)
Multiple threads merged: please forgive chronology errors and repetition 🙂
Jewelry mfgr. needs info about electro-cleaning and electro-polishing process
and Chemical Polishing
of Metals in
Research and Industry"
by W.J. Tegart
-- hard to find & expensive; if you see a copy cheap, act fast!

on Amazon or eBay
or AbeBooks
(affil link)
Q. Hello everyone,
I am a jewelry Manufacturer Based in Mumbai(India). Basically I was looking for mechanized Polishing and cleaning techniques and any of those machines available. Moreover I want to know about electropolishing and electro-cleaning. These are several machines available for polishing gold jewelry but they are media based. I would be more interested in electro-polishing and electro-cleaning. Can anyone give me more information about these processes? Or any person who will be more helpful in this field replies will be appreciated.
Thank you,
Amit [last name deleted for privacy by Editor]Jewelry manufacturer - MUMBAI, Maharashtra, India
2003
A. ELECTRO POLISHING & CLEANING IS POSSIBLE ON GOLD BY REVERSE CURRENT TECHNOLOGY IN ELECTROPLATING.
SACHIN KHARATMALMfg.ELECTROPLATING PLANT & MACHINERY - MUMBAI, MAHARASHTRA, INDIA
2003
Electropolishing of single gold crystal
Q. Hello,
In order to electropolish a Au (111) I use a cyanide solution (ammonia, KCN, H3PO4, K4FeCN6), and I'd like to know if it's possible to electropolish gold crystal by an other way or other solution.
Thanks in advance best regards,

Stephanie Boussert
PhD student - Barcelona, Spain
2004
Electropolishing Au/Ag white gold for bio-system
Q. Hello,
I am a student majoring in material science and engineering at Johns Hopkins University. Recently, I started working on electropolishing white gold (Ag/Au alloy 11 K) to use that as substrate for building a bio-system. I need to get a mirror-like smooth finish. I am currently trying out recipes from a few patents - Thiourea ⇦ on eBay or Amazon [affil link] base solution and potassium cyanide base solution. I tried out the recipes different ways. However, the surface still looks worse than before polishing. I would like to know what people commonly use to make shiny white gold jewelry in jewelry industry. I am thinking that the different reaction rate for gold and silver might result in the rougher surface. Do you have any idea on this? I look forward to your advice.
Thank you!
Young-Ju Kimstudent - Baltimore, Maryland, USA
2004
Q. Now, I use non cyanide electro-polishing solution for gold. But I don't know about it. I want to know about composition of solution, mechanical polishing and other suggestions.
UBONRATH [last name deleted for privacy by Editor]JEWELRY - BANGKOK, THAILAND
2005
2005
A. Yes, there is non cyanide solution for polishing gold and silver.
adv.
Consult us if you need consultation.

Anna Berkovich
(ed. update July, 2025: sorry, Anna has retired)
⇦ Tip: Readers like to learn from others' situations;
some readers skip abstract questions.
Q. I'm trying to find out more about the chemicals and current density requirements for electropolishing of gold.
Thank you.
Mark YeomanContinuum Blue Ltd. - Lingfield, Surrey, United Kingdom
2005
-- appended to this existing thread by editor.
⇦ Tip: Readers like to learn from others' situations;
some readers skip abstract questions.
Q. Could you do us your favour. We wanted to know what solution/chemical will be required for Electropolishing of Gold Ornaments. Constituents of Electropolishing Chemical/solution and its percentage. Its detailed procedure.
Regards.
- New Delhi, India
2005
2006
Q. I would like to put down a question based on Gwynne Edson's patent in 1986 on EP of gold alloys [Ed. note: See topic 82]. I think these questions will also help to answer some questions about general EP, which I am involved in particularly on CoCr alloys and stainless steels. My primary goal here it to understand the chemistry of EP so that I can improve processes that I use for EP of steels and other alloys.
Gwynne mentions that to EP gold alloys (and Cu and Ag) one needs thiourea, urea, a reducing sugar and an activating acid. My question is firstly what is thiourea, and what is its role in EP. Why does one need a reducing sugar and an activating acid. Does one need the acid to create conductivity of the solution? Gywnne also mentions that unfavourable oxidation can occur, could such reactions be responsible for deposits one sometimes sees on the surface of the workpiece. What is the role of the reducing sugar in this. What is the role of Thiourea
⇦ on
eBay
or
Amazon [affil link] in these redox reactions?
My background on EP is from a metallurgists point of view, where we know that there is a window where EP occurs, outside of that window one gets pitting or etching. Also it is recommended in texts that chemicals containing heavy atoms such a glycerol or perchloric acid be used to stabilise the so called anodic layer which is postulated to form on the workpiece. How do these theories connect with the role of reducing sugars and activating acids discussed in Edson's patent.
Finally a commercial question, this work was obviously patented because it was perceived to be of commercial value. Why has EP not been more widely used as a finishing process for jewellery? It seems logical to me that EP is more attractive than mechanical polishing. Are there problems practically that I am not aware of?
Thanks!
Research Engineer - Cape Town, South Africa
A. Hi Janet. Regarding why electropolishing isn't used on jewelry instead of mechanical polishing, I think the resulting surfaces are not as reflective because on a small scale the surface is wavier. Electropolishing is apparently excellent at dissolving asperities and generating a surface more like ocean swells than the plowed ground of mechanical polishing. But once you're down to that swells stage, I think electropolishing lacks the capacity to level them out to an optically flat surface because there isn't a significant difference in current density, nor anything else, between the crests and troughs of those gentle swells. Whereas, if you mechanically finish, you can level out those swells and can get a very flat surface even if, at a very small scale, it's full of clods and plow lines.
Regards,

Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
Need quick confidential answers? $25
Need project assistance? $100/hr.
Electrocleaning vs electropolishing of gold jewellery
Q. Hello, myself from India, a goldsmith. New to electroplating in my work. Bought a rhodium pen plating and gold 24 kt solution from reputed brand. How to clean my rings? I searched the net and get to know about electrocleaning. My problem is whether electrocleaning is different from electropolishing? Does electrocleaning cause gold loss? I am using soft white tip. Nobody near me to help answer my queries. Grateful if answered. Thanks.
Padmanava Jethygoldsmith - Cuttack, Odisha, India
January 11, 2012
A. Hi Padmanava. Electrocleaning should not cause gold loss. Electrocleaning is about using electricity to separate water into hydrogen gas and oxygen gas, and making use of the formation of the resultant gas bubbles on the surface of the part to help 'scrub' it clean. Hydrogen bubbles forms on the cathode, and oxygen bubbles forms on the anode; and such electrocleaning can be done at either polarity.
Regards,

Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
Need quick confidential answers? $25
Need project assistance? $100/hr.
A. Electrocleaning is different
Electrocleaning: using degreasing powder and cleaning it with current.
Electropolishing is totally different, which cuts metal, helps in polishing Jewellery (reduce polishing/buffing process and saves metal loss).
business person - Mumbai, Maharashtra, India
October 24, 2021
⇦ Tip: Readers like to learn from others' situations;
some readers skip abstract questions.
Q. Please tell me the chemicals required to make up the solution of electropolishing for gold jewelry I really need it as soon as possible.
Mr. Asif- Karachi Pakistan
May 6, 2016
and Chemical Polishing
of Metals in
Research and Industry"
by W.J. Tegart
-- hard to find & expensive; if you see a copy cheap, act fast!

on Amazon or eBay
or AbeBooks
(affil link)
A. Hi Mr. Arif. Please introduce yourself and your situation. In the USA and much of the West, such solutions are usually trade secret & proprietary, and purchased from suppliers -- people invest months or years to develop robust metal finishing processes, and then they sell the mixtures rather than the secret.
If you are not experienced in this field and are attempting home-brew, there may be at least two problems we warn you of: First, your initial efforts may result in etching the gold rather than polishing it, which could cause expensive loss of gold. Secondly, most of these solutions involve the deadly poison cyanide -- are you trained and equipped to work safely with cyanide?
One formula printed in "Gold Plating Technology" by Reid & Goldie, which they attribute to "The Electrolytic & Chemical Polishing of Metals" by Tegart is:
Potassium cyanide 65 g/l, Sodium Potassium Tartrate
⇦ on
eBay
or
Amazon [affil link]
15 g/l, Phosphoric Acid 18 ml/l, Ammonium Hydroxide 2.5 ml/l, Temp. 50-60 °C, Voltage 8-10.
Luck & Regards,

Ted Mooney, P.E. RET
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
Need quick confidential answers? $25
Need project assistance? $100/hr.
Non-cyanide electropolishing of gold
⇦ Tip: Readers like to learn from others' situations;
some readers skip abstract questions.
Q. Electropolishing methods: describe non-cyanide gold-density solutions for current and voltage.
Thank you.
teacher - tehran-iran
May 12, 2017
Q. Hi, all masters of electropolishing: Please tell me the voltage for electropolishing non-cyanide gold in the thiourea bath.
Thank you very much.
teacher - thran-iran
June 6, 2017
Q. Dear sir, I have a problem while doing operation of pink gold of 18 kt. I have used all parameters; I used new compound for electropolishing. But there is no results at all. I try it for 50 mins. Please reply to me as early as possible, it's a kindly request to you.
Thank you
Jewelry machine supply - Mumbai, Maharashtra, India
September 20, 2017
A. Hi cousin Amar. Hopefully a reader can help you, but I don't see enough information here to assist you. Have you successfully electropolished pink gold before? Have you successfully electropolished other gold before? Have you successfully electropolished anything else before?
What voltage & current density were applied? What can you tell us about the composition of the electropolishing solution? What was the temperature & pH? Who did you buy the process from, and why aren't they helping you? Thanks!
Regards,

Ted Mooney, P.E. RET
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
Need quick confidential answers? $25
Need project assistance? $100/hr.
September 2017
Sorry! Finishing.com is temporarily Read-Only.
Please maintain your bookmarks! Although Ted Mooney is retiring, finishing.com is not!
It will have a new owner/curator very shortly!