What's So Special About Cadmium Plating?


Q. Hi I need help!

What is the use of Cadmium? What is so special about it? We do a nickel, cadmium, gold plating series. We now want to do away with cadmium. What can we use in place? Core metal is aluminum alloy 60601 - T6 IAW ASTM B209.

Susan Snow
- New Hampshire
2001


A. Leaving out radiation control, the features that make cadmium attractive are: good corrosion resistance, solderability, cathodic protection of steel, galvanic compatibility with aluminum, excellent lubricity, freedom from stick-slip when torquing, malleability, economy, and no gummy and voluminous corrosion products.

However, it is unusual to plate nickel and then cadmium on a part. When it is done it is usually for the purpose of making a diffused nickel-cadmium coating which is a rather different thing than cadmium plating. Nickel plating straight to gold plating is a more common finish, but I wonder if the cadmium layer is intended to sacrificially protect the nickel or aluminum, or maybe discourage mold. It's pretty important to try to find out why it's there before deciding it isn't needed :-)

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
2001


2001

A. Cadmium plating is wonderful. I want all landing gear on every plane I ride to NOT have a substitute for cadmium, NiCd, chromate conversion coating, etc.

I still don't get why we have to eliminate cad and chrome, and I am a card carrying tree hugger. (Keep hard chrome on those chain saw blades too!) All we have to do to waste treat the effluent from the plating shops, and we are done.

tom pullizzi monitor   tom pullizi signature
Tom Pullizzi
Falls Township, Pennsylvania


A. Here's why NASA doesn't like Cadmium plating:

1. Cadmium is known to sublimate in a hard vacuum environment (especially at temperatures above 75° C). The sublimation products, which are conductive, can redeposit resulting in short circuits. The sublimation products may also interfere with sensitive optics.
2. Cadmium is a toxic material that should not be used in manned space flight applications
3. Cadmium is subject to the spontaneous growth of Cadmium whiskers. The propensity of Cadmium to grow whiskers appears to be lower than that of zinc and especially tin. Cadmium whiskers (like tin whiskers) grow spontaneously and are capable of causing electrical failures ranging from parametric deviations to sustained plasma arcing that can result in catastrophic short circuits. See prohibition against pure tin plating for additional insight regarding the risks of metal whiskers.

I also think that when it's exposed to certain types of radiation it becomes extremely toxic, emitting a deadly gas. I heard long ago that a nuclear devices' potential for rendering an area uninhabitable can be enhanced by covering the device with cadmium. Items sold to the government are prohibited from having cadmium plated parts for this reason.

Shawn Barnett
- Shingle Springs, California
2003



2003

thumbs up signThanks, Shawn. Good points, all . . . except your last sentence, which isn't true. There are countless military and aerospace parts that must be cadmium plated per military spec. In fact, if you research the scandal which resulted in passage of the Fastener Quality Act, I think you'll find that the heart of it was that the military felt lives were endangered because some plating shops substituted zinc and zinc alloy plated fasteners where cadmium was specified.

Cadmium is certainly unsuitable for many applications, and it is a cumulative poison we are all working to get out of the environment -- but we can't substitute anything for cadmium without a design review of each individual component. Rather, we need to re-examine, for that particular component, how important good corrosion resistance, solderability, cathodic protection of steel, galvanic compatibility with aluminum, lubricity, malleability, freedom from stick-slip when torquing, and freedom from gummy and voluminous corrosion products is. Nothing has all of the properties of cadmium (if it did, it would be cadmium of course), so we need to figure out which are vital and which are less consequential or of no importance for the particular part.

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey




Difference between tin plating and cadmium plating

Q. I believe some bar stock I am working with is cadmium plated. It's solderable, and there are advantages in that. Does anyone here know of a test to differentiate between "bright tin", and cadmium?

Jim Canale
manufacturing - Tully, New York
March 3, 2009


A. Hi, Jim. The majority of cadmium plated work receives a yellow chromate, which wouldn't be mistaken for tin. Letters 31938 and 38853 suggest spot tests for cadmium. Good luck.

Regards,

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
March 4, 2009



Q. Thanks! Do you know of anyone making small test kits of the chemicals necessary to make the tests? We try to minimize the amount of hazardous chemicals and reagents we have in house.

Jim Canale
manufacturing - Tully, New York
March 11, 2009


A. Hi, Jim. Although there may be a few such suppliers, your local metal finishing chemical distributor will be familiar with all of them, and is always your best best for small quantities because they stock locally and are often able to split orders. If your company buys no plating chemicals yet, so you are unfamiliar with this, look in the yellow pages of your town or the nearest city for a local plating supplies distributor. Good luck.

Regards,

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
March , 2009




Q. We are a supplier of Oilfield Equipment and our customer needs ASTM A193 GR B7 Studs and Nuts with Cadmium plating. Why do they need cadmium plating,
what is the difference between Zinc and cadmium?
Your explanation will be very useful for me,

Thanks and Regards

Palavesam Subramanian
- Dubai, U.A.E.
March 16, 2009



"How Lead, Mercury, Arsenic, and Cadmium Harm Our Health"

on AbeBooks

or Amazon

(affil link)
March 18, 2009

A. Hi, Palavesam. Please see my response to Susan (the 2nd entry on this thread). Your customer may decide to change the spec for the coating after considering the toxicity of cadmium, and you are encouraged to ask him to review the situation; but zinc is not a proper substitute for cadmium in some cases because of lower malleability, incompatibility with aluminum, stick-slip problems on fasteners, and gummy corrosion products. Good luck.

Regards,

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey



Q. Ted, what is a suitable substitute for cadmium plating in automotive applications (we are striving for 20-year performance in our trucks....)

Is "cadmium plating" a good choice for automotive? -- I always understood that if it has cadmium plating, it's going to be quite costly....

Do you have a rough feel for how much more costly cadmium plating should be, compared to yellow or clear zinc?

Thanks,
Jeff Bonn

Jeffrey Bonn
- Springfield, Ohio
April 27, 2009


A. Hi, Jeff. Auto manufacturers do not use cadmium plating anymore and you probably should not either. A zinc alloy like tin-zinc or zinc-nickel may be appropriate but, as mentioned, you need to look at which properties of cadmium you need and to select a replacement coating that offers those particular properties. You can't find one single plating that will replace all cadmium applications. Nothing has all the properties of cadmium. If something had all the properties of something else, it would be that other thing :-)

At one time cadmium was very cost competitive with zinc. The only thing to say about the cost of cadmium now is that it is on an upward trajectory as it gets harder to find. Good luck.

Regards,

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
April 28, 2009


Q. Ted,

You mentioned you don't see many reasons for plating both Cadmium and Nickel on the same part, yet Nickel (usually Electroless) is quite often applied as an underplate on Mil/Aero Aluminum based Electrical connectors and accessories that are top coated with Olive Drab Chromate over Cadmium. What would be the benefits of the Nickel under the Cadmium? And doesn't the galvanic potential between the two create corrosion issues?

Thanks,

John van den Enden
- Toronto, Ontario, Canada
June 10, 2009


A. Hi, John. I don't think that's exactly what I said, but cadmium offers sacrificial protection to nickel just as it does to steel, so I don't see a galvanic issue. I am not familiar with the connectors in question, but sometimes the cadmium and olive drab is required for camouflage color (and perhaps for fungus resistance? -- I'm not too familiar with that aspect).

Electroless nickel is an extremely corrosion resistant, highly conductive, barrier layer finish. To plate onto aluminum requires either cyanide copper or alkaline electroless nickel after the zincate, so it's a question of choosing between the two than choosing to do electroless nickel or not do it.

Regards,

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
June 11, 2009




Q. I am making a small bracket that requires military part number to be stamped or etched (the part is Cadmium plated). We prefer to Laser Etch instead of stamping, but I am wondering if any toxic fumes are produced when Cadmium plating is etched by laser marking?
Can anyone tell me if this is true?
Thanks

Sam Rearick
- Apollo, Pennsylvania
October 4, 2009


A. Hi, Sam. I would expect the cadmium plating to vaporize from the heat of the laser, if you are actually digging into the metal rather than simply blackening it with Cermark or something like that. So I would not suggest this operation unless there is fume removal capacity in the system.

If good provision is made for fume removal, though, I wouldn't think it would be a big deal though. Cadmium is a powerful biocumulative poison, but it's not plutonium, and in the old days muffler repair shops would burn off cadmium plated bolts and brackets, probably releasing several times as much fumes, without formal fume extraction systems.

Regards,

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
October 6, 2009


A. Cadmium is a ductile, very malleable metal. The metal is soft enough to be cut with a knife, and it tarnishes in air. It melts at 321 °C and soluble in acids but not in alkalis. It is similar in many respects to zinc including Galvanic Corrosion protection capability but it forms more complex compounds.
High exposures Cadmium occurs with people who are exposed to fumes and when people breathe in cadmium fumes it can severely damage the lungs. Physical contact to cadmium is harmless. Still cadmium is one of the metals on the ''black-list" which should theoretically mean "zero-option". However, attempts in various countries - notably Sweden - to ban its use have been unsuccessful since it has been recognized that for certain applications there is no immediate substitute. Products and components of products used in aerospace, mining, "offshore" and nuclear fields where lubricity, ductility and resistance to hydrogen embrittlement is sought.

Whilst allowing the use of cadmium to continue for applications where there is until now no proven substitute available, still regulatory authorities are vigorously pursuing stringent targets on discharge limits.

In many cases this is surely causing platers to think carefully about the financial consequences of continuing to offer cadmium since new investment in effluent plant will be inevitable. Cadmium would be a good choice of coating material for parts in contact with aluminum. choice of cadmium plated fasteners for assembly of aluminum airframes in the aerospace industry.
Cadmium does have some specific application and capabilities but where alternate material can be used it is better to avoid its use.

Vijay

Vijay Vijayaraghavan
- Adelaide, South Australia, Australia
September 22, 2010




Q. I'm a car guy that has developed some fixes for my British car that I share with the small community of like owners. I make these parts because I have the time and ability, and sell them to owners that have neither time or ability. I've developed rubber parts and rebuilding of mechanical parts as well.

In this case, I'm developing a remote trunk unlock system that uses a cable (like a bicycle brake). The latch was originally cad plated and items I get for rebuild are generally slightly rusted or missing the cad plating.
I purchased a nitric acid-4%/cadmium-0.1% mixture from Grainger's and need to know how to plate these small items - about 3" x 2" in size. I have low voltage power supplies available.
What's the voltage? Anode/cathode material (which is which?) Time in tank? Dilution of the purchased mixture necessary? What do I add to get the gold/yellow/green color?

Any help would be appreciated by the Jensen Healey community around the world ! THANKS.

Pete Bahr
- Moorestown, New Jersey
January 20, 2011



A. Hi, Pete.

There was a time when lead was used in paint & gasoline, and Mercurochrome & mercury thermometers & mercury treated hats were a commonplace, and cadmium was plated onto miscellaneous auto items, and hexavalent chromate conversion coatings of gold/yellow/green were fairly widely used. But those uses are all history because of toxicity.

Cadmium is plated only by a few plating shops today, and basically only on some exotic legacy aerospace applications; and even this will be short lived. Regular blood tests and other medical monitoring are required. Similarly, hexavalent chromate conversion coatings are a rarity (especially after Erin Brockovich [affil link to Amazonaffil links]) and European RoHS requirements, with almost all shops having converted to proprietary trivalent chromium conversion coatings.

The cathode is the component that you plate onto, the anode is the chunk or slab of metal you are dissolving in order to plate out. Electroplating is a reduction process, and you will find it troublesome to electroplate from an oxidizing acid like nitric acid. Although it is easy to do electroplating as a simple science lesson (see our FAQ: "How Electroplating Works"), robust electroplating on rusted components is not a simple process. However, Eastwood offers a tin-zinc plating kit.

They also offer a paint designed to imitate the color of cadmium, Eastwood "golden cad" [affil links]. This may give you an acceptable iridescent yellow color. Good luck.

Regards,

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
January 20, 2011



January 20, 2011

Q. Hi Ted,
Thanks for the quick response, but I was hoping for it to be a bit more positive.... I'm and old school guy, but as an EE, I had a staff of ME's and Chem E's to work out the plating issues (we never did Cd or Chromate Conversion coatings). Back in the days, we used dilution to prepare the laboratory's effluent in preparation for discharge from the facility. I'm aware of industrial risks, as I've worked with 50kV, megawatts of RF energy and even machining/sanding Beryllium metal in the past. I survived all that, with (and without) the help of OSHA so I figure I can handle the Cad -- yes, I did read the MSDS!
I'm aware of the Eastwood offerings, but the guys that buy and trade my kits know me to be a real nit-picker and I'd like to say that the bits were prepared to the original factory conditions, and not just painted to look like it. Cad plating plus the Eastwood overspray would be OK.
I was hoping that the Cd in the bottle of Grainger solution could be used to plate-out onto my parts, which have been sandblasted to bare metal (steel). Also have "stuff" to clean the parts with prior to plating.
Bottom line is the material I have just will not do the job--correct?
Again, thank you for the info and recommendations,
Pete
BTW, you have a GREAT website!

Pete Bahr [returning]
- Moorestown, New Jersey


A. Hi, again.

The test solution which you mentioned, besides being based on nitric acid (which oughtn't be electrolized because that generates NOx gasses), is too weak for utility by a factor of a hundred. Commercial plating solutions based on cadmium cyanide are available from any plating supplies distributor (as are some cyanide-free processes), but even with your wall full of experience, they may be unwilling to ship to you for fear of liability--you can ask. Established plating shops are subject to so many EPA and OSHA regulations that a vendor can be confident that the buyer has had yearly Hazmat training, wears proper PPE, has an emergency preparedness plan, etc. I know that you only want to buy a very small quantity; I'm just explaining why it may be hard to find a vendor, despite them being in every large city.

In truth, if I were a chemical salesperson, I would not sell cadmium to a hobbyist, not only because of potential accident liability but because cadmium is a bioaccumulative poison that the Air Force is spending millions of dollars annually trying to remove from the remaining life-critical applications, and authenticity of restoration just isn't a life-critical application. But not everyone is as concerned; I believe you can still find this poison on some brake linings :-)

A large library will have electroplating texts with a chapter on cadmium plating, explaining the interrelationships of the variables; access to Mil specs for cadmium plating is free (https://assist.daps.dla.mil/quicksearch/). If you are far more patient than me, you can probably find operational parameters on the net on this site or others, a nickel and dime at a time. Thanks for the kind assessment, and good luck.

Regards,

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
January 21, 2011

----
Ed. note 5/23/13: Make that quicksearch.dla.mil/ now



Q. THANKS GENTS. CAN I NICKEL PLATE SOME AIRCRAFT HARDWARE TO KEEP THE CADMIUM CONTAINED AS I HAVE ENOUGH TOXIC METAL IN ME ALREADY.

EDWARD SCHRADER
AIRCRAFT HARDWARE - NAMPA, IDAHO, USA
November 6, 2011


A. Hi, Edward.

Just about anything is possible, but it's probably a bit difficult to remove the chromate and activate the cadmium plating without destroying it. If you don't need the cadmium, and if you have a willing shop, you can just pass the hardware through a standard pretreatment sequence and it will remove the chromate and cadmium. Good luck.

Regards,

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
March 10, 2012



Q. I have a question on cadmium plated steel part. Plater has told us that if the cadmium plating is exposed to acid, that it will release cyanide gas. I am working with a customer that wishes to bond cadmium plated steel to steel using a two part methyl methacryalate adhesive (MMA). This adhesive does outgas acrylic acid (small amount) would this create an issue of releasing cyanide gas? I would be surprised, since the finished plating would not have unstable cyanide laying around in the plating. Thanks for your help

David Herrick
- Fort Wayne, Indiana, USA
September 13, 2012


A. Hi David.

I can't imagine any realistic basis for this worry.

Regards,

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
September 13, 2012



A. You mean : "if cadmium plating BATH is exposed to acid, it will release cyanide gas" I guess.

Best Regards ;)

Francois Pignon
- France
September 18, 2012



thumbs up signThanks Ted and Francois. You confirmed what I thought, that acid exposure to plated parts is not an issue. Francois, thanks for your comments on acid exposure to the bath. Since this is finished part that is plated, does not look like any issue.

David Herrick
- Fort Wayne, Indiana, USA
September 20, 2012




Q. I am presently working on a cad/chromate line and looking for reference books SPECIFICALLY on the topic. My personal library has most of the books that have a chapter or two on the topic, but I am surprised I cannot locate anything coming close to exhaustive.

Any cad platers want to weigh in on the topic?

The line is an acid cad and major chromate focus is OD.

bob adams
Bob Adams CEF
Tijuana, Mexico
February 22, 2013



A. Hi,

It's the protection from corrosion. If you heat treat cadmium and nickel together you have the the best corrosion protection.

Regards

Anders Sundman
Anders Sundman
4th Generation Surface Engineering
Consultant - Arvika,
Sweden

First of two simultaneous letters -- -March 4, 2013



Q. No takers on the reference materials for Cad and OD so far. Is it that hard to find? I have had no success.

A big issue is blotches in the OD after Cad at the moment. I've tried numerous pre-dips with and without temp. Oddly where ever the blotch is, it is shinny and the rest of the part is more flat in appearance. As I am working with acid cad, I am told that the organic film is hard to break through. Interestingly the best results are either LCD plating or a dilute piranha solution (very dilute), which points back to organics. A 1/4 % nitric dip will uniformly change the surface of the part before OD, but there can still be blotches. I'm down below 1.5% brightener presently and the parts still have a matte luster and I can plate up to 40 ASF with no burning.

Anyone step right in on this one.

thanks

bob adams
Bob Adams CEF
Tijuana, Mexico
Second of two simultaneous letters -- March 4, 2013



A. Hi Bob. I don't think a whole book was ever written about cadmium plating and, since its usage has been steadily declining for 50 years, I don't see any prospect that one will ever be written. One suggestion I can make is Metal Finishing Information Service in England (http://finpubs.com). They have abstracted all of the plating journals for several decades, and offer the abstracts as a CD-ROM, or online, or they will do the search for you -- whatever is your preference. I've used them many times over the years, and find it easy and inexpensive.

Regards,

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
March 5, 2013




Q. I have some small parts made from 1215 steel. Calls for Cadmium plating. What is the purpose of cadmium? Is there a substitute for Cadmium that offers the same results.
Thanks, Tim

Tim Strubberg
- Union, Missouri
February 3, 2014


A. Hi Tim. This thread lists the many reasons that things may be cadmium plated, and the special properties that cadmium offers. It also explains that only very rarely are ALL of those properties required. If all are required, there obviously is no substitute.

If only some of the properties of cadmium are required, there is a substitute -- but which substitute that will be will depend on which of the properties are important. The most common substitute is a zinc alloy plating like zinc-nickel, zinc-cobalt, or tin-zinc. But again, these do not have all of the properties of cadmium plating and it is dangerous to guess which properties were important to the designer. Only the design authority can answer your question about a substitute. Sorry.

Regards,

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
February 2014




RoHS exemption for cadmium is soon to expire -- so what about high voltage contacts?

Q. I have a question regarding the cadmium exemption 8b-for RoHS. Soon this exemption will expire unless the industry can present data for the extension. I have discussed the issue with multiple people and the discussions have lead to the determination that cadmium is irreplacable in high current/high voltage applications where other materials break down causing a welding of contacts to shut and possibly cause a fire. There are several alternatives to cadmium but is there a study that shows where the alternatives do not work and cadmium is the only solution?

Rick Morrison
- Plano, Texas
June 23, 2014




Damaged cadmium plated threads

Q. I have a large threaded bolt which is CAD plated. Some of the threads were damaged and it appears the CAD plating came off. How hard is CAD plating and can it come off threads when damaged? thank you

bill darrell
- amityville, New York, usa
November 14, 2014


A. Cad is very soft compared to steel and is hard compared to lead or solder.
Yes, it can be damaged when the threads are damaged. If it chipped off, then the adhesion was not excellent. It could have passed QC testing and still chipped.

James Watts
- Navarre, Florida
November 14, 2014


A. Hi Bill,

Cadmium is very soft, that is what makes it good on threads!

You have two choices for repair, either strip and re-plate or, if the damage isn't too bad touch up cadmium (MIL-STD-865 is a good place to start for that process)

Brian Terry
Aerospace - Yeovil, Somerset, UK
November 17, 2014




Q. Hi,

I was trying to find a suitable substitute for cadmium coating used in application where corrosion resistance is of primary importance. Lubricity and system contact with aluminium are also some specific features that I was looking for.

Akshay Saraogi
- Gurgaon, Haryana, India
July 11, 2016


A. Hi Akshay. I think you should investigate whether tin-zinc alloy plating will meet your needs. But if good compatibilitiy is actually required you are limited to cadmium plating or plating/coating with aluminum.

Regards,

ted_yosem
Ted Mooney, P.E. RET
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
November 2016




Is cadmium plating always RoHS incompatible?

Q. Can we consider that Cadmium plated fastener parts are always Non RoHS Compliant based on below interpretation :

According to the EU Commission, plating and coatings are homogeneous materials.
And if Cadmium is the single substance in that homogeneous material (plating) then its ppm level should always be beyond the permissible limit of RoHS.

Please advice ASAP. Thanks !!

Neeta Verma
- Delhi, India
November 4, 2016


A. Hi Neeta. I think your syllogism is valid :-)

Regards,

ted_yosem
Ted Mooney, P.E. RET
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
June 2017




Q. Can you cadmium plate aluminum?

dave colbert
- lavergne, Tennessee usa
June 23, 2017


A. Hi Dave. No question that it can be done. But few plating shops have the chemistry and capability to do plating on aluminum, and few shops do cadmium plating anymore. Finding a shop that offers cadmium plating on aluminum might be a chore, and Google ain't what it used to be (it used to display only pages which contained every word and phrases you entered, so 'cadmium plating on aluminum' would do the trick, it's harder these days).

Regards,

ted_yosem
Ted Mooney, P.E. RET
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
June 2017




Q. I have some small parts of 1215 Steel that I need to have CAD plated. The parts have picked up a small amount of rust over the time I've had the parts. Is there a step in the CAD plating process that will remove the rust or will I need to do it myself before sending out for plating?

Thanks, T

Todd Olson
- St. Paul, Minnesota USA
September 5, 2017


A. Hi Todd. The plating shop does all necessary cleaning and acid activation (rust removal) before the cadmium plating step, and chromate conversion coating afterwards. You probably need to specify the thickness of plating and the color of the chromate. Good luck

Regards,

ted_yosem
Ted Mooney, P.E. RET
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
September 2017




Q. I have a round part that is .004" undersize and it calls for a Cadmium plating; is it possible to apply a coating .002" per side on this part to bring it back into spec?

Mark Blenker
- Kaukauna, Wisconsin USA
March 1, 2018




(No "dead threads" here! If this page isn't currently on the Hotline your Q, A, or Comment will restore it)

Q, A, or Comment on THIS thread -or- Start a NEW Thread


Disclaimer: It's not possible to fully diagnose a finishing problem or the hazards of an operation via these pages. All information presented is for general reference and does not represent a professional opinion nor the policy of an author's employer. The internet is largely anonymous & unvetted; some names may be fictitious and some recommendations might be harmful.

If you are seeking a product or service related to metal finishing, please check these Directories:

Finishing
Jobshops
Capital
Equipment
Chemicals &
Consumables
Consult'g,
& Software


About/Contact  -  Privacy Policy  -  ©1995-2025 finishing.com, Pine Beach, New Jersey, USA  -  about "affil links"