Passivation with citric acid


Dear Sir. I work for a small shop in Ohio. We make a part out of chromecore that has to be passivated with citric acid.We are having a problem finding someone who can do this in production. Any input would be great. Thank you,

Kenneth W [last name deleted for privacy by Editor]
- Ohio
1998



Ken there are suppliers out there that are selling Environmentally friendly citric acid based passivation solutions.

They are easily accessible and easy to use.

Mike H [last name deleted for privacy by Editor]
- Philadelphia, Pennsylvania
1997



1997

Ken,

Be careful if you plan to use the citric acid product yourself. Even though it is being marketed as environmentally friendly, it is a strong chelate. If you can batch treat you are o.k. because theoretically all that's in the solution will be free iron, but if this stuff is added to your waste stream it will tie up any metal including copper that it comes in contact with, and will increase your treatment cost and time.

The marketing tool these guys should be using is the safety factor in eliminating nitric acid from your operation, not the environmental angle.
Good luck, Mike

Mike M [last name deleted for privacy by Editor]
- Philadelphia, Pennsylvania



There seems to some strong marketing in the USA of citric acid as a passivating agent.

However, since citric acid is not an oxidising agent, I fail to see how it can effectively passivate stainless steel.

The ASTM A380 a recommended chemistry is nitric acid.

Supposed environmental safety should not outweigh the technical issues.

We would recommend using nitric acid and then neutralise with soda ash or equivalent.

What are your thoughts?

John H [last name deleted for privacy by Editor]
Callington Haven
1998



1998

Dear Kenneth:

citric acid passivation is a tried and true solution to a lot of the problems in the stainless steel industry.

First, it is both safe to use AND environmentally safe when used as directed. Products on the market using citric acid have been thoroughly tested and found to equal or exceed the passivation produced by nitric acid formulae. Because it is a chelant, you do not mix large quantities into the heavy metal precipitation process, but there are ways to handle that very effectively, and many can eliminate the NEED to treat for heavy metals by the use of citric products.

The specification to use for passivation of stainless steel is ASTM A967, not ASTM A380 , which is recommendations, not a spec.

You do not need an oxidizing acid to passivate stainless steel. You need FIRST to remove the free iron from the surface and in inclusions, then let the oxygen in the air take care of the oxidation of the surface. Stainless steel is self oxidizing in air, as long as you are able to get rid of the iron corrosion from the surface.

The proof of whether it works is in the test data, and there is much test data to show how well it works while being safer and lower cost.

lee kremer
lee kremer sig
Lee Kremer
Stellar Solutions, Inc.
supporting advertiser
McHenry, Illinois
stellar solutions banner



I certainly agree with all of what you have said, Lee -- but where is this 'much test data' that you refer to? Can you reference a published article or two for us?

Ted Mooney, finishing.com
Ted Mooney, P.E.
Striving to live Aloha
finishing.com - Pine Beach, New Jersey
1998


Hey! I think I'm going to do a science experiment on the effect of citric acid on the passivation of stainless steel, or something like that. I'm only in ninth grade and I was wondering if I could conduct an experiment on this safely and correctly. It would also be helpful if you could give me some information about citric acid and its effects. Thanks!

Liz R [last name deleted for privacy by Editor]
- Columbia, Missouri
2000


My department invests a small amount of money in pollution prevention projects. A potential proposer has described a project to test a citric-based passivation system to eliminate nitric acid and reduce acidity of sewage discharges.
Two questions: Is this really something that needs to be researched or is convincing info out there(where?); 2) If it does need demonstrating, how many (ballpark) different samples would need to be passivated this way to be meaningful?

Thanks for any views on this.

Tom K [last name deleted for privacy by Editor]
NY State Dept. of Economic Development - Albany, New York
2000


hello sir,

i just have a quick question on passivation with citric acid . We plan to do passivation on a continuous line oven and we are not sure on the percentage, or molarity of the solution of citric acid we should use. the volume of the reservoir in the oven is 1000 gallon, and this volume will be transferred from zone to zone, 5 zones in all. normally in the states we use a 2% nitric acid solution by volume, and basically we are looking for the equivalent using citric acid . if you can help me that would be great. I'm sure you are busy with real customers but this would help me tremendously.

Thank you.

Josh j [last name deleted for privacy by Editor]
- moscow russia
2000



I am interested in your answer to the Liz Roberts question from Columbia, MO. I am also involved in a science project about the effect of citric acid s on Metal. If you do not have an answer, could you please refer me to someone or some website that can help?

Thank you,

Patrick M [last name deleted for privacy by Editor]
- Fairfax Station, Virginia
2000


none
www.finishing.com is made possible by supporting advertisers ...
this text gets replaced with bannerText
spacer gets replaced with bannerImages



(No "dead threads" here! If this page isn't currently on the Hotline your Q, A, or Comment will restore it)

Q, A, or Comment on THIS thread -or- Start a NEW Thread

Disclaimer: It's not possible to fully diagnose a finishing problem or the hazards of an operation via these pages. All information presented is for general reference and does not represent a professional opinion nor the policy of an author's employer. The internet is largely anonymous & unvetted; some names may be fictitious and some recommendations might be harmful.

If you are seeking a product or service related to metal finishing, please check these Directories:

Finishing
Jobshops
Capital
Equipment
Chemicals &
Consumables
Consult'g,
& Software


About/Contact  -  Privacy Policy  -  ©1995-2025 finishing.com, Pine Beach, New Jersey, USA  -  about "affil links"