finishing.com logo ips1
HOME FAQs BOOKS JOBS: Help Wanted Suggestions      you are here: Hotline/Forum => Letter 8074

EN on NiCr

+

I am being asked to electrolessly plate Ni on a NiCr sputtered alloy. I have tried an 30% HCl dip to strip off the native oxide but the EN won't initiate. The features are small, 3 uM openings through a spun on resist pattern. I have also tried a buffered HF solution (10:1) to expose the Ni in the NiCr alloy but to no avail.

Suggestions anyone?

Patrick Franklin
Indigo Systems - Santa Barbara, California


+

Try next:

(1) Reverse etching in sulfuric acid for 60s,switch polarity and
(2) Direct etching for 30s
(3) Reverse for 30s
(4) Direct for 10s.

If you have Nickel strike, plate 2-3 min. rinse and put in EN

Reverse mean parts is connected to positive pol on rectifier

Mico
- Vancouver


ANSWER or FOLLOW UP POST an unrelated QUESTION HOT Topics

Disclaimer: It is not possible to diagnose a finishing problem or the hazards of an operation via these pages. All information
presented is for general reference and does not represent a professional opinion nor the policy of an author's employer. The
internet is largely anonymous; some names may be fictitious and some recommendations may be deliberately harmful.

If you are seeking a product or service related to metal finishing, please check these Directories:

Jobshops Capital Equip. & Install'n Chemicals & Consumables Consult'g, Train'g, Software Environmental Compliance Testing Svcs. & Devices Used & Surplus