How to strip plated silver off copper

+

I am looking for a system that doesn't involve cyanide, nitric acid or machining to strip plated silver off of copper, so that the copper can be reused and replated in needed. Thank you, Peter

Peter Slade
electrical controls mfgr. - Horseheads, NY


+

Dissolve 4 oz/gal sodium nitrate in concentrated sulfuric acid. Electrostrip with a lead cathode at 3V, 70-120F.

totter James Totter, CEF
- Tallahassee, Florida


++

I am looking for a solution to strip plated silver from copper powder (30~40 micrometer), so that the copper can be reused and replated in needed. Thank you, very much

Gyu-Sik KIM
- Asan, ChungNam, KOREA


++

James Totter's reply is essentially applicable, Kim; however, remember to develop this process in extremely small batches until you are familiar with it because conventional plating and stripping chemistry proceeds so rapidly on powder (because of it's tiny mass and huge surface area) that reactions can be virtually explosive.

pic of Ted Mooney Teds signature
Ted Mooney, P.E.
finishing.com
Brick, New Jersey


+++++++

Hi,

I would like to remove silver plating from copper and brass items and collect, I have seen these systems and can not find the manufacturer, do you know who produces this type of equipment.

Thanks,
Mike

michael coletta
- Rockville Centre, New York, USA


July 31, 2008

would like to remove silver plating from copper and brass items and collect, I have seen these systems and can not find the manufacturer, do you know who produces this type of equipment or how to do it without harsh chemicals

kathryn mueller
artist - edwardsville, Illinois


ANSWER or FOLLOW UP POST an unrelated QUESTION HOT Topics

Disclaimer: It is not possible to diagnose a finishing problem or the hazards of an operation via these pages. All information
presented is for general reference and does not represent a professional opinion nor the policy of an author's employer. The
internet is largely anonymous; some names may be fictitious and some recommendations may be deliberately harmful.

If you are seeking a product or service related to metal finishing, please check these Directories:

Jobshops Capital Equip. & Install'n Chemicals & Consumables Consult'g, Train'g, Software Environmental Compliance Testing Svcs. & Devices Used & Surplus


Home    -    Contact    -    ©1995-2012 finishing.com     -    Privacy    -    Search