48515
Passivated parts came back melted
[Connecticut]
April 15, 2008
I had a plater process A.I.S.I. 416 threaded rods to AMS-QQ-P-35C,
Type 1. The parts came back melted. Is This the right specification
for Passivate or should I use type 2?
Brian Gamache
Director Of Operations - Bolton, CT, USA
April 22, 2008
Brian,
Looking at my old copy of Mil QQP35C, it directs 416 SS to be
passivated with Type 2. Of course, Type 1 was removed from the C
revision of QQP35.
I have another chart here, which I believe is based on a combination
of those from QQP35B and QQP35C, which calls for Types 1, 2, 3, or 4
for 416 SS.
Of course, I would be remiss if I didn't point out that citric acid
passivation will never etch or "melt" your parts.
The best rule, perhaps, is to use what gives you the results you want
and don't use whatever gives you results you don't want.


 |
|