we are in the process of doing the stainless steel cloloring
works. Mix of H2SO4 (d=1.84)of 490g/l and CRO4 of 250g/l at the temp
of 70 - 90 degree C.
We only can get 4 relative color so far; with the "blue" "gold" and
"violet". But my question is that is it the only colors I can get by
using this Inco method?
Please guide me here and hope I can get the help I needed!
Teck Lau
stainless steel coloring - Sibu, Sarawak, Malaysia
March 20, 2008
Try next solution:1 lit sulphuric acid/7,5 gm potassium
bichromate.Lead cathode,70-95 C/1,3 V-0.06 a/dm2.5-50 min.
immersion.Brown-blue-redbrown-purple-green colour sequence.Only for
18/8 SS!Hope it helps and good luck!
Goran Budija