45052
Components of electroless tin plating on
piston [Japan]
May 9, 2007
One of my endusers is electroless tin plating on piston for 2/4
wheel vehicle. My enduser just gave me as follows: 1. Dosage of
Sodium Stannate 80 g/liter, dip the pistons in the bath for 60 - 70
seconds, temperature of the bath is 80Ž. My user want us to
instruct how to use our Sodium Stannate including the components of
the bath. Since my company is tin salts manufacturer, we have little
knowledge of plating in details. Please help me on this subject.
Takao Matsui
Tin Salts Manufacturer - Osaka, Japan
May 11, 2007
In my opinion, the honest attitude is the most helpfull to your
customer. Tell him what you have told us, that you are not platers.
He must find a professional plater for good quality and troublefree
service. Of course, you can sell the plater your tin salts.
Guillermo Marrufo
Monterrey, NL, Mexico
May 26, 2007
Gentleman,
Using sodium stannate for Plating on to Aluminium Pistons is called
Immersion Tin coating and not electroless plating.
you have to use 5% of Tin salt in water at a temperature of 80 to 85
degree centigrade. Just immerse the pistons, you will find a coating
of Tin in 2 minutes.Then rinse and dry.
But the free caustic content in the bath should never exceed 5.0
gram/litre. For this the Sodium stannate should contain less amount
of sodium Hydroxide for good control over the bath solution. Or else
Blisters will appear on plating due high caustic content.
Thankyou,
SHANKARANARAYANAN N
- Bengalooru, Karnataka, India


 |
|