Pitting in bright silver anodizing  

++++++

I am inquiring about bright silver anodizing on aluminum extrusions
We have had problems with bad pitting on the aluminum, we bring the metal in from china and have had that blamed but when we push the anodizer it gets done properly.
can you tell me why this happens.

Jeffrey James Stokes
aluminum partition systems - Sydney, NSW Australia


++++++

Suspect chloride contamination in the line. Look for it in the deox, anodizing solution, and seal. IF the parts are racked on titanium and the seal tank is stainless steel, the galvanic current aggravates pitting, then in the presence the chloride pitting will be worse.

Robert H Probert
Robert H Probert Technical Services

Garner, North Carolina

Editor's note:    
   Mr. Probert is the
   author of
Aluminum How-To / Aluminio El Como


Dear reader

Post an answer
 
Post a question
 
Report broken links


Legal disclaimer boilerplate button

List of Directories
Jobshops Directory button Environmental Directory button Equipment Directory button Consultants Directory button Chemicals Directory button Test Directory button Help-Wanted Directory button About Advertising button Classifieds Directory button Booklist button

 

Link to Del.icio.us button Save This Page (why?)    -    Home    -    ©1995-2009 finishing.com