Letter 35081

Anodize thickness  

+++++

The blueprint general notes states:

HARD ANODIZE PER Mil-A-8625 [link is to spec at TechStreet], TYPE III, CLASS 1

What is the thickness required by the spec?

Thanks in advance.

Dennis Millat
Aircraft parts - San Diego, Ca., USA


+++++

I strongly suggest you obtain a copy of the standard.
The default thickness would be .002" +/- .0004 unless otherwise stated on requisition document.

Bill Grayson
- San Jose


+++++

Paragraph 3.7.2.1 under Type III coatings states " Unless otherwise specified ... the nominal thickness of the coating shall be 0.002 inch"

Chris Jurey
Luke Engineering & Mfg. Co. Inc.

Wadsworth, OH


Dear Reader, please --

Answer or follow-up on this subject (in non-commercial fashion).
 
My company is a supporting advertiser at finishing.com and we want the contact information to reach the inquirer privately.
 
Post a new question or inquiry on a different subject.
 


Legal disclaimer boilerplate button

List of Directories
Jobshops Directory button Environmental Directory button Equipment Directory button Consultants Directory button Chemicals Directory button Test Directory button Help-Wanted Directory button About Advertising button Classifieds Directory button Booklist button

 

Link to Del.icio.us button Save This Page (why?)    -    Home    -    ©1995-2009 finishing.com