Hull Cell Equation [Chile]
++++
For Hull Cell I need an equation to find current density at
diferent distances of cathode.
HECTOR LONGUEIRA
- ANTOFAGASTA, II region, CHILE
++++
Hi Hector,
This is the formula to calulate current density for an hull cell
panel.
c=i(5.1-5.25logx)
c= current density
i= current applied
x= distance to be measured on the panel.(panel side close to anode is
hcd area and side away from anode is lcd area)
|
|
Venkat Raja
plating supervisor
Walkerton, Ontario, Canada
|