Hardness in Electroless Nickel plating 

-

Hardness in ENi deposits Is the thickness of the deposit a factor for the as plated hardness of Electroless Nickel ? We plate mid-phosphorus nickel to 0.0005®, is this enough deposit or do we have to go higher ? Thank you in advance.

Enrique Segovia
- Monterrey N.L. Mexico


-

The thickness of the nickel has no effect on the hardness on the nickel. But you get problem using a gauge to control the hardness. Because you must go in beside on the nickel layer for receive a good resultat and that be a problem with a thin nickel deposit. The hardness depend also if you use a heat treatment after electroless nickel. Regard,

Anders Sundman
    surface finishing engineer
Sweden


-

What hardness do you intend to get? The high phosphor EN has a higher hardness than mid phosphor. Heat treatment increases hardness but decreases ability of the deposit to withstand NSS test.

 
Sara Michaeli
    chemical process supplier
Israel


-

Enrique, A mid-phos electroless should give about 38 to 42 Rockwell C as deposited. When trying to get any characteristic from an electroless bath, whether it be hardness, corrosion resistance or wear resistance, you should really be looking at a 1.0 thou or 1.0 mil thickness. Otherwise, you just get the hardness of the base metal. Ray

Ray Delorey
- cambridge, ontario, canada


Dear Reader: please choose what you want to do.

I want to post a question or inquiry of my own.
 
I want to answer or follow-up on this question publicly
 
I am a supporting advertiser and want to reach the inquirer privately.

 





     

 Save This Page (why?)    -    Home    -    ©1995-2008 finishing.com