Formula for titanium electropolishing
++++
RE: Titanium I'm interested in a generic formulation for electropolisihng or bright dipping of Titanium.
Louis HirbourChemical supplier - Anaheim , California, USA
++++
Chemical polishing of titanium:
6o-62% Perhydrol(Hydrogen peroxide)
8-10% Hydrofluoric acid
3o-31% water
temp. 2o C,3o-6o min.
Good luck!
Goran Budija- Zagreb, Croatia
++++
The method you suggest is damaging for the environment and workers. There is a proprietary method of polishing titanium in saline-based solution. Contact us if interested.