How to place the fasteners and shafts in salt spray test chamber  

++++

Hello,

Painted panels can be hanged in test chamber but I would like know the standard practices of positioning the fasteners & motor shafts in the salt spray test chamber?

Prasanna N.
Q.A. - Aurangabad, Maharastra, India


++++

SAE/USCAR-1 requires that the orientation of the primary axis of the fastener to be 25 +/- 3 degrees from vertical. I recommend that you obtain this standard, as it describes the proper procedure for testing fasteners, and it is suitable for shaft components as well.

Toby Padfield
Automotive module supplier - MI, USA


++++

Painted panels should be tested at a 15 - 30 degree angle. For other parts, the significant surface should be a 15 - 30 degree angle whenever possible. Position the test specimen to minimize solution collection in crevices.

Cynthia L. Meade
- Sylvania, OH, USA


Dear Reader, please --

Answer or follow-up on this subject (in non-commercial fashion).
 
Post a new question or inquiry on a different subject.
 


Legal disclaimer boilerplate button

List of Directories
Jobshops Directory button Environmental Directory button Equipment Directory button Consultants Directory button Chemicals Directory button Test Directory button Help-Wanted Directory button About Advertising button Classifieds Directory button Booklist button

 

Link to Del.icio.us button Save This Page (why?)    -    Home    -    ©1995-2009 finishing.com