Preserving heat coloring of copper when clear coating

-

I have tried all forms of heat (oxyacetylene, electric oven and home stove top gas) to produce the effect seen on this butterfly refrigerator ornament, but cannot duplicate the vivid colors.


Courtesy of Mel Owen

Since I have 2 of these I assume it can be duplicated. Is another ingredient ( oil?) added or is it a matter of a consistent temperature?

Mel Owen
- Texas


-

Chemicals might have been required to achieve this. Maybe you could borrow a copy of Colouring, Bronzing & Patination of Metals [link is to product info at Amazon] and see what you think.

pic of Ted Mooney Teds signature
Ted Mooney, P.E.
finishing.com
Brick, New Jersey


.

The coloring produced on the butterfly can be done with heat. You don't have to slather your work in harmful chemicals to get some great coloring. You have to experiment like never before and work with the heat from any torch and "paint" the copper with the flame. You can try working with oils as well. I once was annealing some brass in a kiln and I took it out too soon for annealing but the oil from the factory must have still been on it because it produced some amazing colors and patterns.(The pieces of metal were framed and hung in 'Out of Hand Gallery' in Lunenburgh, Nova Scotia!) Grease may be easier to work with than oil. You have to play a lot with the torch because it is easy to heat the metal too much and the colour will go to a yucky brown. Also try working with folding the piece and annealing it. When you open the work you get some interesting colour patterns due to the amount of oxygen that gets to the metal in the folds.

The trick is to play! Have fun and ALWAYS WEAR PROPER SAFETY GEAR! PROTECT YOURSELF AND YOUR ENVIRONMENT!

M.Jardine
- farmington, nova Scotia, Canada

Basic Copper Smithing and Flame Painting on Copper

Rent the DVD:


++

I HAVE NO PROBLEM GETTING THE COPPER TO CHANGE TO ALMOST ANY COLOR. This is the copper after heating it.

My problem is losing all the blue,red, and purple colors, When I apply any product to keep the copper from tarnishing. The other photo is after the product is applied.

I have applied a large variety of products and none have worked to my satisfaction. I will be very pleased for any advice you can offer.

SONNY GRAHAM
- OZONA, FLORIDA


+++

Yes, I have the same situation as Sonny. I have tried spraying the heat-colored copper with clear Krylon or lacquer, but it seems to oxidize beneath the surface of the clear sealer (about 6 months later). How can I preserve the heat-produced colors without having oxidation? I also often have a roughened, sanded surface, so I'm not sure if wax would be an option.

John Waters
- Phoenix, Arizona


Unfortunately, I don't have good news for you, Sonny and John :-(

Some portion of the nice coloration is from diffraction patterns like the rainbow sheen of a drop of oil on water, rather than from pigmenting. The oil isn't really rainbow tinted, it's the way the very thin layer prisms the light. As soon as you put a clear coat on your piece, it's like trying to lay a sheet of glass over that oil rainbow to preserve it. The colors that are "really there" as pigments will be retained, but the diffraction colors disappear.

pic of Ted Mooney Teds signature
Ted Mooney, P.E.
finishing.com
Brick, New Jersey


+++

Try using OIL-based polyurethane instead of lacquer. Or another oil-based product.
The problem with water based products and many of the lacquers which are acidic is their reach with the copper creating another patina, not necessarily he one you want.
I have not tried this with colors like yours, but I've used it on both bare brushed copper and sulfurated potash patina copper ( mostly dark colors) and it preserves most of the color.

I have a copper dining set I made about 7 years ago and it's still pretty much same color (that picture is when it's about 4 years old).

I just experimented with several brands and price does not seem to make a difference. Cheapest worked same. Polyurethane also has the advantage of being flexible, unlike lacquer, which will have hairline cracks after a while for temperature expansion and shrinking of the copper and will lose it's protection.

I've tested it by bending a coated piece back and forth and them leaving it in salt water for a month with no visible tarnish while the lacquer piece turned black.

Alik Perakh
- San Diego, California


+++

I am a hobbyist working on a table top project looking for a way to treat copper. I am looking for a dark rainbow swirl effect and nobody has been able to help. I also would like to know what to use to seal it after this affect is achieved.

Jeri Bond
hobbyist - Syracuse, New York


++++

Please tell me where I can find help. I want to heat 110 copper sheet .032 gauge .. I want to bring out areas of orange, yellow, red, etc. What common tool can I use and how hot should it be? Is there a website, article or book that you can suggest? THANKS BUNCHES

Dottie Cesario
hobbyist Tampa, Florida


++++

I've managed to produce a wide range of hues on copper with an ordinary propane torch. The trick seems to be in heating the copper to a high temperature and then using the torch as you would a paint brush. Heat one portion of the piece until color starts to appear and then experiment. A long time under the torch close to the heart of the flame produces pale greens, silver, and gold. A quick stroke with the edge of the flame produces blues. A longer time at the edge of the flame produces reds and pinks.

Joe Nicholas
- Kansas City, Missouri


++++

I am a hobbyist making copper wind chimes. I am burning the copper chimes with a propane torch to bring out the different colors in the tubing. When I put a finish on the pipe, the colors fade and and some colors, like purple, disappear completely turning to orange. I've used lacquer, Rustoleum products, shellac and a variety of water based (acrylics) clear finishes used for hobbies and purchased at hobby stores all with the same results. Does anyone know of any kind of finish either brush on or spray that will not change the oxidation of the pipe.

Tony Wright
hobbyist - Huntington Beach, California


++++

We are trying to create a tropical sunset scene in sheet copper and would like to embellish the work primarily in blue and red hues. A metal worker mentioned applying bromide salts to the metal prior to heating with a propane torch. Has anyone had any success with this method? Any other recommendations?

Thank you!

Bob Yeamans
- Columbus, Ohio


++++

I would like to know what process I need to employ in order to discolor either copper or brass. I believe what I want to do is etch the metal, but I don't know what chemicals to use or possibly how to heat it to accomplish this. I'm working on a a logo which will be large and want to use discolored and/or distressed metal. Any help you can offer will be appreciated.

Thanks

Paul

Paul Le Pain
artist - Dunedin, Florida


++++

I have had great success keeping the blues, purples, and reds in my flame treated copper. I worked with my local powder coater and found that a clear finish baked at half the time usually required, does the trick. It allows the powder to melt to a clear glaze and give the copper a depth that spray on treatments don't allow, but by leaving it in half time,the copper doesn't heat up too much to change color.

Emily Lewis
- Burlington, North Carolina


+++++

I am interested in what you have discovered re: coloring of copper with varying temperatures. For a different reason, though. My apron front copper sink was damaged, and it had a "Fire and Ice" finish on it that was beautiful. It had to be polished off during the repair, and I would like to replicate all the colors that were represented. (I realize I can't replicate it exactly.) Thanks for any info!

Peggy Thomas
- Amarillo, Texas


+++++

Hi

I am trying to preserve the color on HEAT patinated copper. I have tried water based Incralac, paste wax, spray lacquer, Krylon 1301 [linked by editor to product info at MisterArt]. The best results have been the Krylon. However it still changes the color. Do you think that a solvent based Incralac will work better at preserving the color? Thanks for you input.

Bruce MacKimmie
- Moss Beach, California


+++++

I would like to know the best way to bring out color in brass using a blow torch. Should I use something in addition to heat. Also, what is the best way to keep the colors? Should I polyurethane it? I want to make art objects with copper and get the beautiful purples and golds from the heat.

Lynn Schmoock
hobbyist - Hillsborough, New Jersey


+++++

I have tried many things to ensure that my copper fountains remain nice and shiny waxes and acrylic finishes. But unfortunately of all of them the worst thing I have found is putting a lacquered finish on them. Whether it's the combination of outside elements or the water or both I don't know but it begins to discolour after a couple of months and the finish begins to really look drab.

I am experimenting with a company in the UK that works with clear powder coating, and I am trying to get something that is ok to use outdoors with water over a long period. It might be a while till I get a decent result but if it works I'll post the info later in the year.

Craig Humphreys
- London, UK


++++++

I create metal sculpture for patio and poolside with 18 gauge sheet metal. I'd like to add random color (blue and whatever other hue possible) to the sculpture using my oxy-acetylene torch. How is this achieved and what settings do I use on my regulators? Have looked for books on the subject, but can't find any.

Polly Fisk
metal artist - Dallas, Texas


++++++

Hi. I make penny whistles from copper and heat color them. I have had very good luck finishing them with Brass Lacquer. It is formulated for brass and copper and works well. It is somewhat costly, but it works. Look for it on ebay, sometimes you can find a good deal.

Rick Hinck
- Holyoke Colorado


++++++

I was trying to form an oxide film on copper by thermal oxidation at 350 deg.C, in ambient atmosphere. After 10 minutes, there was a gray film on copper, which I assumed was CuO. After about an hour at 350 deg C, the surface became multicolored with patches of pink, violet and gray/black! What are the possible compounds that cause these colors?

Nandini Venkataraman
Student Researcher - Tucson, Arizona


++++++

Getting red from copper with a torch. I am new to coppersmithing and have been trying to get the color in my leaves and butterflies when I cut them out with the torch. Does anyone know how to do this? Is it in the regulator settings or what? I have tried everything.

Jeremy Whitmire
coppersmith - Copper Country, Michigan


++++++

How do I use potash to color my copper project? I'd like to find out what the application is and how and what do I mix the potash with?

Ross D Laird
Primal Iron Originals - San Diego, California


+++++++

When I do small projects on copper, I usually get a nice fire-scale effect by "painting" the parts I want to color up with flux (flux for hard solder), letting it dry, then turning the piece over and heating it from the back.
I usually heat it pretty hot to get a nice red color, but keep the flame away or it'll burn the flux and turn a funky color. Use the flux lightly...

Jessica Schafer
- Santa Cruz, California


+++++++

If you want to turn copper red heat it as hot as you can get it without melting it then dunk or spray it with water. When I make a rose from copper this will make a very bright red rose.

Lyle Wynn
blacksmith - Flowood, Mississippi


+++++++

I understand the problems of losing colors after heat coloring. I do steel coloring. The best way is to use cold roll steel. After you obtain the effect you want, leave it set over night or longer and let it cool down. Then I use a spray called EnviroTex high gloss =>

Hold the can at least 18" from the piece working on and spray a light coat. Let this dry and then do the same thing again. Do this several times but DON'T GET TOO CLOSE. You might lose just a little lighter blues but the deep blues and purples will stay. Also the clear powder coat will work at half the baking time. When the powder starts to glaze over I shut the heat off and pull the piece out of the oven There is a new low heat clear powder coat coming out. Don't have the info on it yet.

Mike LeMaster
welding - Delta Colorado


January 24, 2008

Hey, I do a lot of heat coloring on all kinds of metals,the best thing I have found is Renaissance wax [linked by editor to product info at Amazon] it's a micro-crystalline wax polish.It's a little expensive but the best thing I found that leaves a natural finish (not shiny glossy).It does "tone" down the colors a little bit(depending on how/when u apply) but if done right NO color is lost.

Frank Bachmann
- Glen Burnie, Maryland

Renaissance Micro-Crystalline Wax Polish
Renaissance Micro-Crystalline Wax Polish

 


January 25, 2008

As we all know, if you put a drop of oil in a puddle of water you will see a colorful rainbow sheen. The rainbow colors are not the color of oil, they are an interference pattern or diffraction pattern that results when light encounters a very thin film of transparent material.

Some of the heat coloring colors are real: they are pigments and patinas. But some of the colors, especially the more subtle, are not: they are diffraction patterns caused by very thin films of oil or oxides or something on the surface. The clear coating removes these colors not by chemical reaction or yellowing (alone) or filtering, but simply by being there. If you study the subject of carnival glass (which also gets it colors from diffraction patterns, not pigments) you may find something useful about film thickness, etc., that can help you preserve heat coloration. Just a thought, for what it's worth, from someone who doesn't practice the art but believes based on this that the wax is the best bet.

pic of Ted Mooney Teds signature
Ted Mooney, P.E.
finishing.com
Brick, New Jersey


April 30, 2008

I am fairly new to copper work. I do not use sheet copper, but rather cold forge heavy copper wire. I have been experimenting with different patinas and coloring techniques and am very fascinated with heat coloring. I experimented some using the broiler of my oven and achieved a gorgeous hot pink/purple color. However, as soon as the copper cooled, it faded quickly to orange...a very nice bright orange, but NOT the color I wanted. Is there a way to keep that lovely pink color? I had not seen it before in any finished copper work, so I am very curious if it is just a color that shows up when the copper is hot, or if it is possible to keep that particular shade. Any help would be great appreciated!

Genevieve Lancaster
hobbyist, designer - Atlanta, Georgia


June 10, 2008

I've been working with copper for about 13 years and have gotten some beautiful iridescent-like patinas with Liver of Sulphur [linked by editor to product info at Dick Blick]. It's a benign substance, available in crystal form from any chemical supply house or in liquid form from any garden center -it's the orange liquid part of Dormant Oil Spray that's used to spray fruit trees in late spring and cheaper than the crystals. Liver of sulphur is the substance that smells like rotten eggs (remember stink bombs?), so take care where you use it.

It should be mixed with water and makes a very light brown to black patina, depending on the ratio of water to liver of sulphur. Less water = darker color. I get the nicest iridescent coloration when I apply with a brush. Experiment with different ratios on scrap until you get an effect you like. The effect is instant and if you don't like it, clean the copper and try again. The patina isn't stable so it has to be lacquered after the desired effect is achieved. Additionally, the water mixture loses viability fairly quickly, so only mix what you'll use in a few minutes -30 minutes, tops.

I hope someone finds this useful.

Cheers!

Kathleen Donaldson
- Kingston, Ontario, Canada


May 4, 2009

I am currently a student concentrating in metalwork. I have experimented extensively with heat patinas, and I have learned a number of things that I haven't seen addressed on this thread. I use a propane torch with the broadest tip I can find, the heat should be very general and not focused too much. On larger pieces I even use a rosebud tip. To produce an even color you need to heat the copper evenly and in very small increments. The final color will only come out after the copper has cooled, so pull the torch away and just watch the piece. Colors will develop as the copper cools. If the piece was not heated evenly it will have inconsistent color. The trick that I have learned, and have had extraordinary success with, is air cooling (NOT QUENCHING! submerging in water will cause the color to flake) as quickly as possible. I do this by running outside in the winter and swinging the piece through cold air. You can also stick it in a freezer when you see a color you like develop. Don't sit the piece down on the racks in a freezer, though, it will cause the color to be uneven in the places where the metal touched the rack. Using an air compressor and blowing on the piece is quite effective as well, the compressed air is quite cold. It has taken me many experiments, and many failures, but I am able to pinpoint any color in the color spectrum by heating slowly and evenly, removing heat and observing, and air cooling as quickly as possible. Even though I consider myself quite skilled at applying heat patinas, I still pickle most pieces and start over multiple times to pinpoint the exact color I am looking for, every piece will be slightly different depending on it's size, inconsistencies in thickness, and, sometimes, shape. As far as sealing a color, I have found nothing to be effective, personally I like the idea of an ever-changing piece, if you really want to, you can always clean it up and reapply the patina after it is lost.

Cody Pinnow
- Menomonie, Wisconsin


December 21, 2009

I make wind chimes with flame colored copper tubes. I seem to get better colors by heating the tubes with the torch until the colors just begin to come out then I let it "rest" and cool for just a couple of minutes then hit it again with the torch and really make the colors come out. I also found a product that really seems to work and not dull the colors. It is called X-I-M 900 clear coat. It is designed to protect polished nonferrous metals. I holds up extremely well even outdoors and doesn't seem to dull the colors. I found it at my local professional automotive paint supply company. Its made by XIM Products; they sell it online. USE 3 OR 4 LIGHT COATS. It looks a little frosty at first but quickly dries clear. Good Luck.

Dale Firm
- Canton, Ohio


S
I
D
E
B
A
R

Why does the color of pure copper which is used in Cyclotern change to rainbow color by heating with burner?

Can I make an exact duplicate.

deba prasad dash
employee - Kolkata, westbangal, India


January 12, 2010

Hi, Deba. I would assume that the rainbow coloration is oxides of copper as described on this page. I think making a duplicate is more about artistic skill and experience than scientific understanding of the technology. In other words, I doubt that I could make a duplicate, but I believe that a skilled metal artist could :-)

Good luck with it.

Regards,

pic of Ted Mooney Teds signature
Ted Mooney, P.E.
finishing.com
Brick, New Jersey


October 23, 2010

Hi All.

I work extensively with Niobium and Titanium patination, so I have some info that might help.

The rainbow colors is light diffraction caused by clear oxides. The color is dependent on the thickness of the oxide.

Scientifically, the ratio of oxide thickness to light wavelength determines the final color you see.

The answer is therefore to wipe the flame across and experiment. There is no way to tell exactly how much.

An atmosphere high in oxygen would help. An oxyacetylene torch would be best, with the oxygen turned up high.

Ryan Diederich
- Wilbraham, Massachusetts, USA

February 27, 2011

It is possible to color copper with heat and preserve the colors. I've been doing it since the early 90s. The colors I can achieve are copper, brown, purple, blue, green, yellow, orange, rose, and black. It does however take many, many hours of trial and error.

Verrel Martin
- Fulton Missouri

April 4, 2011

I haven't done much with copper, and I've only used a torch on silver in a class, I didn't seem anyone mention using a heat gun, it's like a super hot hair dryer apparently used for peeling paint, anyway one day I was in my basement and there was the heat gun and a piece of copper, so I turned it on and used it on the copper, it worked very nicely, the copper going through all the color stages as it progressively got hotter, it also seemed very controlled to me. Just thought I'd put that out there!

Logan Swift
- Monmouth, New Jersey, USA

May 19, 2011

I recommend using an oil based lacquer. A few coats is all you really need. If you want more protection, you can spray one coat of lacquer followed by a self-level epoxy that you can pour on the surface. The combination of the two makes the copper really "pop". The plus side of the epoxy is that you can sand it down and pour a new coat on top after a few years of wear and it will look brand new again. Hope that helps.

Don Angelo


Spring Hill, Tennessee


November 26, 2011

I am just starting out soldering copper. I make jewelry. I saw a clasp that I was told was copper with a layer of gold over it, and it had the rainbow colors in various places. Does anyone know what this technique is called and how I can achieve it?

Thank you,

Verlynda

Verlynda Teague
- Charlotte, North Carolina, USA

December 10, 2011

Another reason why your heat patina might not last or look the same as it did is in the nature of the patina itself. If the piece is going to be outdoors the metal will eventually be heated and change color. I learned this from experience. I had this happen with one of my pieces that got left in the car in the summer for a bit. It looked washed out afterward. Besides being in the car nothing touched it, not even direct sunlight.
I've had another piece that I have sitting inside that I did, I haven't put a clear coat on it of any sort and it's fine. The heat patina will last a long time, but it's in no means a completely permanent coloring eventually it will fade and tarnish clear coat or no.

Ashley Blissit
- Lubbock, Texas, USA


ANSWER or FOLLOW UP POST an unrelated QUESTION HOT Topics

Disclaimer: It is not possible to diagnose a finishing problem or the hazards of an operation via these pages. All information
presented is for general reference and does not represent a professional opinion nor the policy of an author's employer. The
internet is largely anonymous; some names may be fictitious and some recommendations may be deliberately harmful.

If you are seeking a product or service related to metal finishing, please check these Directories:

Jobshops Capital Equip. & Install'n Chemicals & Consumables Consult'g, Train'g, Software Environmental Compliance Testing Svcs. & Devices Used & Surplus