Toxic effects from galvanized food preparation utensils
+++
I recently purchased a stamped steel propane barbecue. Upon inspection I noticed that the heat/flame dispersion plate is galvanized. I realize that many studies conclude that galvanized metals should not be used for any type of food preparation, or storage. A Michigan State University web page states,"Galvanized utensils...should never be used for food preparation or storage." The fact that this particular item has obtained standards clearance to the point of sale, has me greatly concerned.
Can anyone direct me toward any other facts concerning zinc toxicity, especially regarding fumes from heated galvanized steel? Any effects, symptoms, or specific guidelines that are relevant to this human health issue are difficult to find, unless it is about avian zinc poisoning.
Any help is greatly appreciated!-Jeff
Jeff Swayze- Kelowna, B.C., Canada
+++A heat/flame dispersion plate is clearly not a food preparation or storage surface where food acids or biological activity could dissolve zinc into the food, Jeff. And galvanized metal is used in all sorts of hot applications which offer some limited potential for people inhaling fumes: automobile exhaust systems, hot ash cans, exhaust flues for furnaces and water heaters, electrical light fixtures, etc. I would certainly expect that the hardware used to assemble the hot areas of a propane or charcoal grill would be zinc plated.
If you don't want to use the grill and you want your money back, just take it back. If you are concerned over the public health, this particular one I would classify as de minimus :-)
A do-it-yourself smoker might possibly be a bigger issue due to the possibility of inadvertently using cadmium plated metal or hexavalent chromated metal, but personally I don't think there is any reason to continue to be concerned about this propane grill, Jeff. If I have misunderstood, please clarify. Thanks.
![]()
Ted Mooney, P.E.
finishing.com
Brick, New Jersey
+++Thanks for the speedy response, Ted! Well I am mainly concerned due to the effects I have heard from welding galvanized metal. Anytime you heat steel there is some gassing and obviously welding galvanized steel is going to cause some really nasty vapours, which contains some zinc, (nitrate), or so I have been told by some welders.
I guess my question is, if galvanized steel is heated to the point where "heat staining" occurs, are these vapours harmful? Can then these vapours deposit zinc nitrate onto food in an enclosed vessel, like a barbecue? Your answer, I gather is likely "yes, but not to any extent to be concerned about."
I am not attempting to de-bunk the galvanizing or plating industry, as my inquiries are based upon university research which has shown that the possibility of zinc poisoning from an item such as the one discussed may be much greater than previously suspected. Due to advances in bioreactive research technology, many items which were once considered safe, are now unavailable to the public.
I imagine that there are varying levels of sensitivity to suspect products from person to person, and to avoid many or all of these products would be impossible.
I appreciate the response and industry-based opinion, and of course, the mindful and candid manner in which you remind readers that there should be a "point" to questions, which I sometimes forget. Thanks Ted!
Jeff Swayze
- Kelowna, B.C., Canada
+++I'm getting old, Jeff, but within my lifetime it was considered medically essential that water never be put on a burn, only butter and other oils. And I can remember when manufacturers of breakfast cereal were, for years, lambasted by media and Congress for subverting our children into a habit of eating the "empty calories" of whole grain and fiber instead of wholesome protein like bacon and eggs and liver. Diet A is labeled worthless and diet B a healthful life style, then the positions reversed, back and forth, almost every other month. Where are we with female replacement hormones -- good or bad? It's changed at least 3 times in 6 months. After half a lifetime of intensive study, is aluminum linked to Alzheimer's or not? Sorry, still debatable. Mammograms good or bad, an alcoholic drink a day good or bad, coffee good or bad, milk good or bad, plastic butcher blocks an important replacement for cracked wood surfaces or an oleophillic surface that guarantees contamination?
We are a paranoid society which places far too much belief in the sketchiest of theories as long as they're scary (Toxic Timebomb in Your Kitchen! - News at 11); they are all instantly accepted and rarely demonstrated. If we can't decide whether carefully monitored things that are ingested daily are good or bad for us, shall we honestly worry about very casual exposure to heated zinc?
What shall we make things of? Better not use aluminum! Steer clear of nickel! Don't use zinc! Copper and silver are powerful biocides that must be avoided. Rusty bare steel, forget it! Chrome? Don't be crazy. Concrete? Silicosis. Wood? Harbors bacteria. Vinyl? Carcinogenic vapors. Asbestos? Get real. Is cobalt safer than nickel? Probably until diets A and B reverse places.
We need to watch the biggies which it is hard to argue the dangers of: mercury, lead, and cadmium. And keep our eyes open for a fourth baddie, and then a fifth. But our government throws money at beltway bandit researchers (campaign contributors) who have been on the road of diminishing returns for decades, looking harder and harder for the slimmest of possible risks to scare us and extend their grants; our politicians make hay "protecting" us from the specter of toxic hobgoblins; and the TV networks keep us watching by warnings of impending calamity. Only an opinion.
![]()
Ted Mooney, P.E.
finishing.com
Brick, New Jersey
+++
I have been exposed to steel rust fume while taking steam bath. What are the harmful effects of such fumes on me?
Dheerah GS- India
+++Bleedin' 'ell, Jeff !
You are only going to get (some) fumes from normal metal products when you go to welding temperatures ... and the welding temperatures are WAY, WAY, WAY higher than a little ole flame or two in a barbeque.
Heck, why not say, ah, Teflon coated frying pans should be forbidden because when you heat Teflon you generate fluorocarbons. True but false. True if the temperature is excessive such as welding around 1300 degrees C, false if you use if for everyday normal cooking.
Ted's answer was very good INDEED....
Worry not ... nor should that Dheerah worry about his so-called steel rust fumes. Just go and enjoy your steam bath ... probably much safer anyhow than bathing in the Ganges, eh?
![]()
Freeman Newton - White Rock, British Columbia, Canada Ed. note:
Please keep Freeman in your thoughts
& prayers.
Message from Freeman, Dec. 2010
+++Hey kids! Well I see the subject did continue on for some time. I have been really busy running a stainless steel sales/ manufacturing/ finishing business, but I did have time to experiment with my barbecue!
My findings are that indeed the piece of galvanized steel AND the other surrounding metal both created some acrid, smelly fumes for about 20 minutes during the first ignition.
After that, all I could smell was some tasty burgers, steak, and wild salmon. My conclusion? Well I'd say light up your new equipment and let it heat up real good once before you toss your fine meats on it, and let your nose be the judge as to when it's been heated long enough. Mmm...I love science!
I hope this will officially conclude this stream and save Ted from having to answer it anymore, because it is silly.
Jeff@HoleJoy!;)
Jeff Swayze
- Kelowna, B.C., Canada
++++Who says scientists don't have a sense of humor? I stumbled onto this thread wondering whether it would be safe to use galvanized hardware cloth (aka screen) to contain small pieces of "real" charcoal in the bottom of my large, black, tripod-legged, kettle cooker.
My hypothesis is that Jeff's approach will work well for me eliminating whatever harmful fumes might otherwise be discharged.
Thanks, everyone!
Patrick Greenwood
- Omaha, Nebraska
+++
We are building a large outdoor BBQ for cooking a whole pig. Some call these Cajun Microwaves. This will have two sections. The first is a rotisserie section and the second is a large shroud. The wood fire is built inside the shroud and the rotisserie section is placed next to the shroud. The shroud's main purpose is to direct the heat towards the cooking pig.
My question is whether it would be ok to build the shroud from galvanized steel. Since this rig will sit outside the galvanized coating would keep it from rusting. On the other hand, I am worried that the heat from the fire may cause the galvanized steel to give off poisonous gases which could contaminate the pig. Is this true or am I worrying about nothing?
John Greeven- Corvallis, Oregon
+++Hi, John.
As you can see from the above, we all have to draw our own lines when it comes to minimal exposures. I probably wouldn't build a pig roaster like this out of galvanized metal because I'd be worried that the material was misidentified and the plating might be cadmium. But that's just me, and I wouldn't argue with someone who felt it was perfectly safe.
![]()
Ted Mooney, P.E.
finishing.com
Brick, New Jersey
+++
Should there be any worry of exposure to hazardous materials when using galvanized metals in applications other than cooking or welding. For example, I've seen a lot of galvanized items at the local Home Depot like nails, framing for shelves...etc. Does the zinc (or cadmium) used in galvanized items like this readily rub off onto your hands or outgas in any way.
Also, how can you tell if a galvanized item contains cadmium? If it does, what safety precautions should be taken?
Thanks!
Tony T [last name deleted for privacy by Editor]- Ramsey, New Jersey
Hi, Tony. I seriously doubt that anything you find in a hardware store these days is cadmium plated. Zinc is not toxic; in fact, it's a vital nutrient, and cold prevention lozenges are zinc compounds. Welders face a special problem in that they vaporize the zinc and then inhale an overdose.
Regards,
![]()
Ted Mooney, P.E.
finishing.com
Brick, New Jersey
+++
Well I have enjoyed the discussion on toxic effects of galvanized steel. My question is in a smoker can you use a galvanized pan to hold the charcoal in the bottom of a drum to cook the hanging product? Will the charcoal , say 5 lbs or ten lbs heat up the pan so much that toxic fumes will contaminate the food products during a three or four hour cycle? The pan I want to use is a large new galvanized oil pan. The juice from the food will drop on the coals and the pan. Will this cause the pan to rust and is it cleanable and reusable? Could this type pan also be used for holding water and seasoning above the lower pan and would that seasoning or gravy be edible? or is........galvanized steel just a bad thing to use anytime with real charcoal and barbecued food.
Thanks,
Lew Orban- Auburn, California
+++
I recently constructed a wood fired BBQ. I made the grill myself out of 8 mm stainless steel rods of unknown grade. I was told by an Australian industrial chemist that, when heated to high temperatures, stainless steel releases toxic gases/substances. Is this true?
Eugene BajadaSchool Lab Technician - Xewkija, Gozo, Malta
++++
Dear All
Go to the "Fact Files" section of the European General Galvanizers Association site at www.egga.com and it will give you the information you need about service conditions for galvanizing.
You can find extensive toxicity info at www.iza.com, the site of the International Zinc Association.
Michael Burcher- Caterham, UK
++++
My Husband and I have been learning how to do blacksmithing projects. At one of the demonstrations one of the blacksmiths made a cheese slicer. My husband and I each mode one, but now we need to place some wire on it to slice the cheese. My husband was going to buy galvanized wire but I didn't think that it would be a safe choice. Is galvanized wire ok for this type of use? Is galvanized wire safe for use with any food items?
Katherine Aprilhobbyist - New Orleans, Louisiana
++++Galvanized wire is probably not a good idea. You should use stainless steel wire, Katherine.
![]()
Ted Mooney, P.E.
finishing.com
Brick, New Jersey
++++
Hi - I want to use galvanized steel to cover a kitchen countertop. Food will probably occasionally come into contact with the surface, however, I will not be preparing food directly on the surface. I like the rustic look of galvanized steel, as opposed to stainless steel. Also, a stainless steel countertop is way beyond my budget. Do you know of any reason I should not use galvanized steel as a countertop? Will it contaminate my food if I set dishes on it, or if food touches it? Thank you so much for any help you may be able to offer.
Nancy Jones- St. Louis, Missouri
++++Galvanized metal is not solid zinc, but steel with a zinc coating -- so it may eventually rust. What would also concern me is the effects on the looks of the counters of acidic foods like vinegar, lemon juice, and tomato juice. They will attack it, and your counters will acquire a "used" look with different shadings from such exposures.
Some people worry about food contamination (www.icat.org.au/documents/cr-2002-09-GIbench.pdf, for example) but I personally felt that report rather silly and wouldn't worry about it myself. Zinc countertops are widely used and have long been. I visited the grand mansions of Newport last year, and in the grandest of them all, The Breakers, as I recall the rows of food preparation and cutting counters were all zinc.
What was good enough for Cornelius Vanderbilt would be good enough for me :-)
![]()
Ted Mooney, P.E.
finishing.com
Brick, New Jersey
++++Hello again.
Thank you so much for your quick response regarding galvanized steel countertops. I agree that if it was good enough for Cornelius' home, it's good enough for me. (I'm sure my humble little house would fit in a Breakers' closet.) Thanks again!
Nancy Jones
- St. Louis, Missouri
++++
Is it safe to grill directly on a galvanized steel grate in an outdoor fire pit? Will it be safer to burn a couple of hot fires first?
Joe Shamma Jr.- Salem, New Hampshire
++++
Good morning, hope you are doing well, a friend of mine is building a cooking box for roasting pigs out of oak and lining the inside with galvanized sheeting that is used in roofing, question is, is it safe or harmful ? Thank you and have a great day.
Juan Correacomputer support - Pembroke Pines, Florida
++++
Wow you just never know what you will find on the internet. I recently was given a 22 pound turkey. Decided to go ahead and cook it. I realized in what. I don't own anything large enough. So I searched around and found what I think is a galvanized pan. Thinking hey, I can line that with foil. And of course wrap my turkey in foil. This will work. That's right I'm no gourmet cook. So you do the best you can. But then this little thought weaseled into my brain. Will this pan put off any poisonous fumes while in the oven. Since my Mom didn't know. The next best thing was the internet. So here I am. I've read everything here.
And most things speak of out door cooking on grills etc. So, sorry to say. I'm still concerned about putting my turkey in this pan in the oven. So Ted if you respond to my concern. Please be gentle. Oh,, and saw your picture. Are you married? :o) Karen in southern Mississippi

Karen Wise
- Natchez, Mississippi
++++You must have read too quick and thought that was my house in the picture four posts above, Karen -- because no one else has flirted with me in about 20 years :-)
But I do have a son who's single and I think he'd be impressed with your pic and your ways :-)
Galvanized items, which usually can be identified by their shiny "spangled" look, are not suitable cooking surfaces. Wrapped in foil your turkey would be fine, so if you've already done it, save a drumstick for me.
But I don't think a galvanized pan should be used in an oven as a rule, because they are not designed for that function; and it's always difficult to predict all of the possible consequences when something is used in an unintended way and we consequently don't have a rich history of experience to guide us.
![]()
Ted Mooney, P.E.
finishing.com
Brick, New Jersey
+++++
I just found this page and would like to post a related question. I have just added a baffle to my offset smoker so it prevents the heat to get directly from the fire chamber to the food, so it redirects it to the bottom of the cooking chamber. The baffle was supposed to be a piece of non-galvanized, unpainted steel (22 gauge), but since I did not find one, I did buy a similar one made of zinc.
Now, after having mounted it, I'm worried it could be toxic. I have read the answers and they make me think using this would be ok, but just to make sure, can you confirm?
Thanks a lot,
- Randolph, Massachusetts
+++++
I have recently purchased a galvanized steel tub of the sort used for watering livestock. It is an attractive addition to my garden that I use as an outdoor bathtub. I want to use it as a hot tub by elevating it with bricks and heating it from bellow with a propane camp stove. What I want to know is, will the heat caused by the stove be so hot that it will burn off the zinc surface on the bottom of the tub? I'm not so concerned about the toxic fumes as this should not be an issue if the flames are not hot enough to burn off the zinc, and if the zinc does burn off in the area above the flames, fumes should be of no concern after the initial burning. My main concern is that the tub might rust and eventually spring leaks in the absence of the protective zinc coating. If this is likely, what other ways might I heat this tub without causing any damage?
Thanks,
U.S. Army - North Miami, Florida
+++++
Is it safe to use galvanized steel lath on a bar b q grill? I was told the heat could cause something toxic to get into whatever is being grilled.
Respectfully submitted,
Roger C. Schustereithobbyist - Cleburne, Texas
+++++This thread is growing long and repetitive, but my own personal comfort level is that I would use such lath to hold the coals in a homemade grill, but I would not put the food on it. For that I'd use stainless steel, or nickel plated or ceramic coated grates.
![]()
Ted Mooney, P.E.
finishing.com
Brick, New Jersey
+++++++
I first would like to say these articles are really helpful. I was just made aware about the "HARMFUL EFFECTS" of galvanized steel and using it for BBQ pits and that it should not be used EVER..and this was from a "Welder" but in my situation it is a 4' 0"" grill for high heat cooking...such as steaks,burgers,fajitas as well as some oysters....i just want to make sure that this will not pose a problem for my guests if I decide to use this grill..i think I have a safeguard in the sense that there is no top so the fumes will not play a factor since I will only have the desired meats on the grill for no longer that 10 minutes tops....i hope this makes sense ..this is my first time on here..Thank you,
Cruz Garzaconsumer - San Antonio, Texas
+++++++
I have built a sauna and the stove is made out of an old propane bottle I use a tiger torch and wood to heat the sauna and the chimney is made of galvanized steel it is actually exhaust pipe that you would use on a bus ( it is however new and has never been used as exhaust) so we heat the sauna up and spray water on the stove and chimney, what are dangers of using galvanized here does the pipe get hot enough? I don't have a temperature reading but I can tell you that the stove and pipe all glow red when it is in use I know people say when welding galvanized the get sick I have used the sauna 1 time and feel fine but I am wondering if people can tell me some info
John Randolfstudent - Vancouver, Canada
+++++++
As President of the local Board of Meals on Wheels, it has come to my attention that the cooks in the kitchen prepare bread dough in a galvanized pan (the size of a wash tub!) and there is some thought and concern of the zinc content in the tub. Does this pose a threat to the recipients? They cannot find a suitable container,they say. There is no heating done to the pan.
Thanks for your quick response.
- Florida
+++++++That should not be done, Janet. See web1.msue.msu.edu/imp/mod01/01600817.html. I know nothing of bakery equipment but am confident that such pans are available tin plated or of stainless steel construction.
![]()
Ted Mooney, P.E.
finishing.com
Brick, New Jersey