Aging solution to give carbon steel coated with zinc a gray aged patina

++

I'm a craftsman and I'm having a hard time finding an aging solution for my creations. I'm wanting to give it a dark gray aged patina. I use a carbon steel coated with Zinc.

Jeffrey Dean
- Lancaster, P.A., U.S.A


+++

Gray for zinc or zinc plated material:

2oo gm iron chloride

1 lit water

Cold immersion(2o min.)!

Good luck! Goran Budija
- Zagreb,Croatia


ANSWER or FOLLOW UP POST an unrelated QUESTION HOT Topics

Disclaimer: It is not possible to diagnose a finishing problem or the hazards of an operation via these pages. All information
presented is for general reference and does not represent a professional opinion nor the policy of an author's employer. The
internet is largely anonymous; some names may be fictitious and some recommendations may be deliberately harmful.

If you are seeking a product or service related to metal finishing, please check these Directories:

Jobshops Capital Equip. & Install'n Chemicals & Consumables Consult'g, Train'g, Software Environmental Compliance Testing Svcs. & Devices Used & Surplus


Home    -    Contact    -    ©1995-2012 finishing.com     -    Privacy    -    Search