HOME FAQs BOOKS JOBS: Help Wanted Suggestions you are here: Hotline/Forum => Letter 17068
Nickel Stripping
++
I would like to get an answer for some questions:
1. I need full description of how to strip electroless nickel from copper? and what type of chemicals and conditions can be used to achieve that?
2. I need a description of stripping of gold?
best regards
Mohammed Omer Jamjoom- Dammam, Saudi Arabia
++
Dear Mr Jamjoom,
For stripping NiP from copper there are commercial strippers on the market. You can try this recipe:
60 g/l Sodium hydroxide
120 g/l Ethylene diamine
60 g/l m-nitrobenzene-sulfonicacid
Temperature 75 C.
About your question for a description of stripping of gold, what's the base metal?
Kind regards,

Sjamp van Esch
- Eindhoven, The Netherlands