Stripper for electroless nickel

--

I am looking for a stripper solution to strip electroless nickel from a 40 carbon alloy steel.

Mandar Sunthankar
- Fort Collins, Colorado


--

We use a product from Fidelity called 3136. It takes about an hour at 200 F to strip 150-200 microinches of high phos electroless. If this seems excessive, you must realize that high phos electroless will show no effect whatsoever after a 30 second nitric acid dip.

This stripper leaves underlying copper plate untouched. It is an alkaline material with nitrobenzoic acids and ethylene diamine so waste treatment is a nightmare. Fortunately we have little need for it most of the time.

I am sure other vendors also have similar products.

Bill Vins
microwave & cable assemblies
Mesa (what a place-a), Arizona



-

Please also see our FAQs on Stripping of Electroless Nickel.

Regards,

pic of Ted Mooney Teds signature
Ted Mooney, P.E.
finishing.com
Brick, New Jersey


ANSWER or FOLLOW UP POST an unrelated QUESTION HOT Topics

Disclaimer: It is not possible to diagnose a finishing problem or the hazards of an operation via these pages. All information
presented is for general reference and does not represent a professional opinion nor the policy of an author's employer. The
internet is largely anonymous; some names may be fictitious and some recommendations may be deliberately harmful.

If you are seeking a product or service related to metal finishing, please check these Directories:

Jobshops Capital Equip. & Install'n Chemicals & Consumables Consult'g, Train'g, Software Environmental Compliance Testing Svcs. & Devices Used & Surplus


Home    -    Contact    -    ©1995-2012 finishing.com     -    Privacy    -    Search