letter 1119
Long term corrosion resistance of
aluminum
Need a salt spray cabinet? ==>
---
I have been unable to locate any hard data on the long term
resistance of certain aluminum alloys in a salt fog environment. We
need a low cost finish such as
Iridite, but able to
withstand up to 5 years in a warm, salty environment. Painting is
expensive. Anodize is OK, but is there a cheaper alternative?
The alloys I am interested in are 2014-T6, 6061-T6, and 7075-T6. I
would like to see evidence of the corrosion resistance of these
alloys after 5 years or more in a salt environment when coated with
Iridite, or anodize, or any other low-cost suggestion. I have an
immediate need.
Bruce Chisholm
Lockheed Martin
---
Bruce:
One possibility is plating the aluminum alloy with high purity
aluminum. This plating acts as a sacrificial anode to any Al alloy
because there are no galvanic sites to initiate corrosion - similar
to the ALCOA Alclad material used in aircraft skins. The plating
takes Alodine or Irridite or other aluminum conversion coatings and a
bolt manufacturer in MI has tested aluminum plated and chromated
steel bolts for over 6,300 hrs in
B-117 [link is to spec at TechStreet] salt spray. Price may
be competitive or not depending on the size/geometry of the parts and
the thickness required, but I thought you should know that plating
With aluminum is available.
F.A. Sandy Donaldson
- Minnesota
---
I would be reluctant to use either 7075 or 2014 in a seacoast
environment even with a protective coating due to the risk of
exfoliation corrosion. 6061 is not susceptible to this type of
attack, but may sustain some minor pitting and surface deposits even
with anodizing.
Look in the literature for references to experiments at Kure
Beach. There has been tons of work there on long-term exposure of
steels with various compositions and coatings to sea coast
environment. There may also be experiments there with aluminum.
|
|
Larry Hanke
materials testing laboratory
Minneapolis, Minnesota
|
---
ASM International has a good handbook which addresses corrosion
behavior of aluminum. It is the ASM Specialty Handbook
Aluminum and Aluminum Alloys [link is to info about book on Amazon],
and they are located at Materials Park, OH. The ISBN is
0-87170-496-X.
Lee C. Branch
---
Thank you all so much for your valuable information. I appreciate
the time you took to respond to my needs.
Of particular help was the ASM International Handbook on Aluminum.
This book has literally everything you need on aluminum, including
the long-term data I was looking for. I highly recommend the book to
anyone with a question about aluminum.
Thank you again.
Bruce Chisholm
Lockheed Martin
-
-
 |