Letter 142
|
|
|
|
Ted, Thanks for the response.
The zinc whisker phenomenon is my reason for being dissatisfied with zinc plating. These microscopic zinc whiskers can cause unexpected failures in low voltage electronic applications.
I could change the surface finishing process from zinc plating to conductive paint, but I think I'll pay a higher cost. What do you think or recommend?
I've read that zinc whisker growth is due to compressive stresses being set up in the plating during the zinc plating process and that stress relieving, heating the part to an elevated temperature after plating has been completed, will relieve the compressive stresses. In your opinion is it true that zinc whisker growth is due to the zinc plating process and that performing a heat treatment to the plated part, after plating is complete, will prevent the whisker growth? If performing a heat treat will prevent the whisker growth, what time and temperature should be used? The base metal is 1 mm to 2 mm thick low carbon steel that is formed to be used as enclosures for AC and DC power supplies.
Also - If the plating process is the cause of whisker growth, what process controls or steps, other than heat treatment, can be put into place to prevent the whisker growth occurrence?
Thanks again!!
Peter S![]()
- Tucson, Arizona
I don't know if you caught the response to Letter #20, but you might find it helpful. I had never heard of zinc whiskers until August '94 when I read the article referenced in Letter #20; few people had.
I believe that internal stresses provide the energy for this whisker recrystallization, due to the presumed parallel with tin whiskers.
I'm even reluctant to reply about conductive paint or other plating's because I don't want to imply that they would not suffer from this same pest when I really don't know.
If there's anybody out there who is knowledgeable on this, give us a hand.
|
|
Ted Mooney finishing.com Brick, New Jersey |
Hello, We all know the causes for metal (zinc) whiskers stresses and temperature but I have yet to see someone providing any experimental results on zinc whisker.
I am hoping to do some experiments on the causes, rate of growth and methods for eliminating zinc whiskers in new parts and maybe reducing existing parts from this monster.
If any have failed parts please let me know. Thank you.
NS
N.Satar
- Toronto, Ontario, Canada
hello, I have a problem with tin whiskers. It is sure that mechanical treatment or heating treatment diminish the occurrence of whiskers growing. In some case, organic coatings used for PCB protection are not enough to prevent that problem. There is an internet site about tin whiskers on NASA Goddard space with experiments on-going.
Christophe Parsis
matra marconi space - France
Hi Christophe
Heat Treatment is just one way to reduce the whiskers but one must be careful it does not alter the properties of the base metal.
N.Satar
- Toronto, Canada
Zinc Plating. My research has shown that the most likely cause of zinc whisker growth is a result of stress build-up during the plating process. Our company has eliminated zinc plated parts on a global scale, and replaced them with nickel plated mild steel, stainless steel or chromate-conversion (Alodine) aluminium.
Tin-lead vs Tin plating with heat treatment. As the whisker problem seems to be related to heat treatment (stress relief), and tin-lead plating of copper is supposed to reduce the whisker growth, does anyone know what the result is if the tin-lead is also heat treated?
Kevin E![]()
- Mulgrave, Victoria, Australia
You didn't say what your product line is, Kevin, so I'll bite my tongue instead of saying: "That's an overreaction!". Remember that chromate conversion coated aluminum has a limited future, and both stainless steel and nickel plating cause allergic skin reactions.
|
|
Ted Mooney finishing.com Brick, New Jersey |
Ted,
Our product line is electronic switching equipment in the telecommunications industry. The change from zinc-plated to stainless steel, nickel plated steel, or chromated aluminium was introduced when some of our older products developed a problem with zinc whiskers causing short circuits on printed circuit boards. The zinc whiskers were being dislodged from surrounding metalwork by cooling fans. I understand that most of the allergy problems that you refer to are mainly associated with the jewellery industry, and I have seen statements that stainless does not leach in the same way as nickel. I would be interested in your comments on this, and the statement about a limited future for chromate conversion of aluminium.
Kevin E![]()
- Mulgrave, Victoria, Australia
|
(2002) Nickel has been proscribed from jewelry in Europe; but it's probably fine for switch gear. I don't think I agree about the stainless, on the general principal that people with nickel itch often find that they can't wear a wristwatch with a stainless back. Beginning in Europe again, there are already strict standards on recycling of automobiles that have forced the elimination of hexavalent chromium compounds on cars. This has been extended to the U.S. more recently and there will be no hexavalent chromate on U.S. autos beginning in 2003 I believe. The elimination of hexavalent chromium has been a continuing effort for decades. I have heard the premise, but am not in a position to test it, that alloy zinc platings resist whiskering in the same way tin-lead resists whiskering.
March 2, 2009 The heat needed is between 135 and 145 degrees. this seems to help but not alleviate the problem Howie Evans
|
|
|